[*] posted on 1-10-2018 at 06:30


At 500C you should have only nitriding with little carbon absorption from the sources I have read.
Nitriding is only a couple of mils deep in most cases again from what I have read.

It sounds like it worked which is rather cool. Now there is a use for the millions of tubes of hardened super glue sitting in everyone's houses.
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 1-10-2018 at 15:50



IMG_2612.JPG - 906kB
Fig.1 The test bodies pre cyanoacrylate treatment

Two sections of mild steel pipe (only one is used in experiment) and a disc of high strength threaded rod center section with the tread machined off. I do not know the exact compositions of the alloys, but the mild steel pipe I trust is mostly iron with less than 0,3% carbon as it is not heat treatable. The high strength threaded rod is definately a high carbon alloy judging by spark test and it definately also contains alloying elements of carbide forming nature (most possibly chromium). It is one of the least machinable steels that I have encountered. It just eats cutting tools....tool steel and carbide alike. It also work hardens to the degree where even honed carbide is unable to touch the surface once it has been hardened by a dulled tool skidding over the workpiece.

IMG_2618.JPG - 642kB
Fig.2 A view into the sodium carbonate filled reaction vessel after 2h in 500C furnace. The cyanoacrylate encrusted samples are buried in the depth of the vessel.

IMG_2621.JPG - 900kBIMG_2623.JPG - 973kB
Fig 3. The samples after the supposed nitrocarburizing treatment. Both look very little affected by visual assessment.

The samples were "scratch tested" with file and showed a slightly increased surface hardness to pre treatment condition. It was still possible to cut both with a file, but a very thin hard surface layer was covering them (supposedly nitride bearing layer).
The mild steel pipe was spark tested and showed a definite high carbon signature. Unless nitrogen inclusion produces the same spark (not that I know of) then there must have been some carbon migration into the samples even under these mild conditions.
The mild steel sample was also subjected to a water quench from around 850C after which the surface of the sample hardened to a degree where it was no longer possible to cut into it with a metal file (most probably a carbon case?).
The high carbon steel sample was not subjected to additional heat treatments as i would not have shown any recognizable effects (it was highly water hardenable already in the pre nitrocarburizing state).








Exact science is a figment of imagination.......
View user's profile View All Posts By User
macckone
International Hazard
*****




Posts: 2160
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 1-10-2018 at 19:18


This is really cool work. Obviously ammonia nitriding would be more reliable than this if you could work with ammonia gas. But the fact that you do get nitriding with the methylcyanoacrylate is cool.
View user's profile View All Posts By User
tocnaza
Harmless
*




Posts: 1
Registered: 2-10-2018
Member Is Offline


[*] posted on 2-10-2018 at 01:02


Very interesting, thanks for sharing!
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 2-10-2018 at 03:16


Quote: Originally posted by macckone  
This is really cool work. Obviously ammonia nitriding would be more reliable than this if you could work with ammonia gas. But the fact that you do get nitriding with the methylcyanoacrylate is cool.


Thanks for the kind words! :)
I'm not totally sure that I get a nitriding action here....it looks more like a carbon enrichment type of process is mostly happening. With perhaps a very slight nitriding because the surface layer of the samples was harder than before the treatment. It is still not nearly comparable to the boriding treatment...that case was epic in it's pure hardness.

I think the main cause for the weak nitriding action is that the gaseous reactants just escape the vessel too quickly and not much interaction occurs. I'm not inclined to use a closed vessel for the process and create a possible rupture in the furnace spilling cyanide gas into the lab. I trust my lab assistant would not hesitate to cast me into concrete for that kind of a stunt :D :D




Exact science is a figment of imagination.......
View user's profile View All Posts By User
rolynd
Harmless
*




Posts: 16
Registered: 13-12-2004
Location: At Home
Member Is Offline

Mood: No Mood

[*] posted on 13-10-2018 at 20:55


According to the vid description this guy is using a mixture of
45g urea
40g potash
10g sodium hydroxide
10g salt
at a temp of 580°c for 1h

https://youtu.be/g91tC6n7jTw

[Edited on 14-10-2018 by rolynd]
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1698
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 14-10-2018 at 02:18


This should create sodium cyanate, making it a fairly standard nitrocarburization-bath.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Texium
Administrator
Thread Moved
27-11-2023 at 12:33
 Pages:  1  2

  Go To Top