Author: Subject: Graphite Substrate Lead Dioxide anode
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 8-1-2016 at 06:20


I was asking about the percolate cell but it is also interesting to know about the plating current density as well.

would it be a problem to have high current density for plating ? I see the PDF uses 5v supply.

View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1358
Registered: 2-9-2014
Location: Technion Haifa
Member Is Offline

Mood: old jew

[*] posted on 7-2-2016 at 09:37
NaClO4


I dont know, what it help us, but here is pretty a new video with clay cup membrane for producing NaClO4.
https://www.youtube.com/watch?v=8ZnYqmbiukI
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 7-2-2016 at 12:40


Thx Liptakov,


Quote:

There are two advantages to this method, you can use graphite as an anode, and you can get 100% conversion due to no cathodic reduction.


I think the video explains the idea of PHILOU Zrealone that he expressed in his thread.

I need a little help now to understand this statement "you can get 100% conversion due to no cathodic reduction" what does this mean ?

[Edited on 7-2-2016 by ecos]
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1358
Registered: 2-9-2014
Location: Technion Haifa
Member Is Offline

Mood: old jew

[*] posted on 8-2-2016 at 01:35


Well, I understand, this: Get 100% change from NaClO3 on NaClO4. It is very important for produce NH4ClO4. Without group ClO3. Or 0,1% ClO3 + 99,9 ClO4. Cathodic reduction (for this type galvanic reaction) is question for PHILOU and others kings of chemistry. LL.
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 8-2-2016 at 06:00


It is quite hard, not to say impossible, to obtain pure perchlorate crops by direct electrochemical means and without any further purification. The resulting cell liquor, even though it mostly contains perchlorate, will still be contaminated by a small amount of residual chlorate. This can be removed by chemical means though:

http://www.oocities.org/capecanaveral/campus/5361/chlorate/d...

Another means is to purify the perchlorate is by heating to convert the residual chlorate impurities into perchlorate and chloride. The chemical means probably is more reliable though...

As a matter of fact the thermal conversion of chlorate into perchlorate is actually quite appealing. Considering the simplicity of the conversion process and the ease with which chlorate can be produced in bulk by the electrochemical method, then it may make sense to omit the hassle of platinum or GSLD and the electrosynthesis route for perchlorate altogether.
Just produce coupious amounts of chlorate by electrolysis of chloride with MMO anodes and heat it to conversion temperature in a porcelain or stainless crucible (preferably with PID temp control). For sure the method is less effective in terms of yield, but way cheaper and quite simple:

http://people.ku.edu/~matt915/projects/chloratedecomp.html

https://www.youtube.com/watch?v=EC4OPnvPkLU

The percursor chlorate must be free of organic or metallic contaminants that may cause a firey explosion or decomposition into chloride and oxygen via catalytic action...







Exact science is a figment of imagination.......
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 8-2-2016 at 12:30


Good post! I have done the research a few times as well, but never got around to trying the thermal decomposition method. It does seem to have a lot of advantages over the electrochemical approach. Yield is a bit low, but so what. It is a relatively quick process, with minimal capital investment in equipment and like you said the chlorate feed is so cheap and easy to make in large quantities.



"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 9-2-2016 at 07:51


Quote: Originally posted by Hennig Brand  
Good post! I have done the research a few times as well, but never got around to trying the thermal decomposition method. It does seem to have a lot of advantages over the electrochemical approach. Yield is a bit low, but so what. It is a relatively quick process, with minimal capital investment in equipment and like you said the chlorate feed is so cheap and easy to make in large quantities.


Thermal method is well known but it is risky. chlorate became very active when heated and any organic existence might end with explosion !
try to avoid it.
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 9-2-2016 at 10:06


Lead Dioxide Electrodeposition Under Ultrasonication : https://www.youtube.com/watch?v=UgYgcymCJ20
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 9-2-2016 at 13:37


Quote: Originally posted by ecos  
Quote: Originally posted by Hennig Brand  
Good post! I have done the research a few times as well, but never got around to trying the thermal decomposition method. It does seem to have a lot of advantages over the electrochemical approach. Yield is a bit low, but so what. It is a relatively quick process, with minimal capital investment in equipment and like you said the chlorate feed is so cheap and easy to make in large quantities.


Thermal method is well known but it is risky. chlorate became very active when heated and any organic existence might end with explosion !
try to avoid it.


I am not saying this to be rude, but driving a car can be extremely dangerous too if one doesn't have the necessary skills. Like driving, I am sure that I could learn to perform this process safely as well.




"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1358
Registered: 2-9-2014
Location: Technion Haifa
Member Is Offline

Mood: old jew

[*] posted on 10-2-2016 at 03:36


To control dangerous processes, that's great art, that's great beauty. Just as God.
Dr. Liptakov
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 17-2-2016 at 09:17


I am thinking to electroplate graphite rod with lead dioxide.
I found two different kinds of graphite electrodes, one is black and one is gray.
$_57.JPG - 109kB $_587.JPG - 115kB
what is the difference between both ?

View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 17-2-2016 at 09:42


The grey rods contain graphite and the black one looks like compressed carbon . . . ?

View user's profile View All Posts By User
Mabus
Wiki Master
***




Posts: 238
Registered: 3-11-2013
Member Is Offline

Mood: Energetic

[*] posted on 17-2-2016 at 13:22


Vitreous carbon maybe?



View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 19-2-2016 at 05:10


i think the difference between carbon and graphite electrodes is the crystal structure of the carbon atom.

would electroplating of compressed carbon rod work for chlorate cells ?
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 25-2-2016 at 09:39


I am ready to build this setup :
Capture.PNG - 64kB

I bought lead , some copper and diluted nitric acid 65%.
I have a fan motor and some beakers.
I think I am ready.

I have a problem now to connect the shaft of the motor with a aluminium rod and to connect the Al rod with the graphite rod.

is there a better way than using glue? I prefer mechanical ways. I wish I find something like a drill chuck that can connect things together with different dimensions.

any suggestions ?
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 25-2-2016 at 11:09


This has worked for me in the past for reasonably low torque arrangements:

Plastic tubing (vinyl, polyethylene), from the hardware store comes in all the standard sizes. The outside diameter of one size is the inside diameter of another. Short lengths of tubing can be used as couplings. If connecting two shafts of different diameters, build up the small shaft with smaller diameter couplings. If the shafts are standard sizes the tubing will fit snuggly like a glove. If friction isn't enough then drill a hole through all (shaft and coupling) and put a pin through, or use an adhesive of some sort.




"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 25-2-2016 at 13:29


Thanks a lot hennig ,

you mean a tube like this ?? :

tubing.jpg - 7kB

I got your idea, this will be between the shaft of the motor and the Al tube.
what about the connection between Al tube and graphite rod?

my problem , I plan to get graphite rods with different diameters (13 mm , 19mm , 23 mm , ..)
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 26-2-2016 at 11:57


You're welcome. There are at least several different types of tubing available at the better hardware stores around here. Even the more basic stores usually have vinyl and polyethylene. Also, a tube with the least curvature is best (outside start of a large diameter roll perhaps). With the two shafts close together in the "coupling" the connection is almost perfectly straight even with tubing with a bit of bend (imbalance of stress from one side of the tube to the other causing curvature). I think this would work with a graphite shaft as well.

The plastic tubing (coupling) also acts as a torsion shock absorber. Depending on the tubing chosen the coupling can be very elastic. This could possibly be a good thing when brittle shafts are involved.


[Edited on 27-2-2016 by Hennig Brand]




"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1358
Registered: 2-9-2014
Location: Technion Haifa
Member Is Offline

Mood: old jew

[*] posted on 27-2-2016 at 03:39


Crisis place in the red circle. If the connection is soft, graphite misalignment occurs. You need hard tube against axis displacement.

cap.jpg - 73kB
View user's profile View All Posts By User
hyfalcon
International Hazard
*****




Posts: 1003
Registered: 29-3-2012
Member Is Offline

Mood: No Mood

[*] posted on 27-2-2016 at 05:34


How about something like this:

https://www.zoro.com/climax-metal-products-coupling-rigid-st...
View user's profile View All Posts By User
Hennig Brand
International Hazard
*****




Posts: 1284
Registered: 7-6-2009
Member Is Offline

Mood: No Mood

[*] posted on 27-2-2016 at 06:04


If it is so soft and so much slack is allowed that it is flopping around when spinning that is a problem of course. However, even relatively stiff polyethylene, which holds its shape well under most normal conditions, has enough elasticity (is non rigid) so that spikes in torsion force are greatly reduced (lowered in amplitude and stretched out). Too soft is of course a problem. Not sure it is even needed, it was just a passing thought.



"A risk-free world is a very dull world, one from which we are apt to learn little of consequence." -Geerat Vermeij
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 8-3-2016 at 02:52


"I think if someone has lead dioxide powder he can add some epoxy and make stiff anode". I read it somewhere but I don't remember the source.

I found a nice clean technique to make lead oxide : https://www.youtube.com/watch?v=Wzm3N0xPyGU

I think if we add lead to a ball mill and run it for long time. the lead will be atomized and oxidized as well. (I think this is the reason why we add 5% carbon while milling Al to cover it and avoid oxidation)

if this will work we could have lead oxide or dioxide and make anodes easily. I am still investigating this point.
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1358
Registered: 2-9-2014
Location: Technion Haifa
Member Is Offline

Mood: old jew

[*] posted on 15-7-2016 at 06:00


As very good idea is clay cap from Philou aparatus. From page 1 this thread. I have questions. Is possible as active surface ( in clay cap garden) use different lead oxides? Thus only pure Pb3O4 - minium? Has the Minium similarly properties (for galvanic process) as PbO2 ? Or worked Pb3O4 only with mix in PbO2? 1:1 ? Is posible used Pb3O4 without clay cap aparatus? Will be worked high pressed rod from Pb3O4 ? Thanks,....LL....:cool:
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 20-7-2016 at 06:14


I have a question.
I found some offers on the internet for crucible graphite. some of them are used and with good price.

anybody know if they can work as electrodes?

$_57.JPG - 119kB
View user's profile View All Posts By User
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 20-7-2016 at 06:47


Quote: Originally posted by ecos  
I have a question.
I found some offers on the internet for crucible graphite. some of them are used and with good price.

anybody know if they can work as electrodes?


Problably, although they might have some additives to make them more suitable for their purpose, I guess.