crazyboy - 11-6-2015 at 18:37

I saw a video where plastics were distilled in an oxygen free environment to make a flammable liquid which was claimed to be diesel like. Here it is: https://www.youtube.com/watch?v=4G34HQQqHRw

This got me interested, I have heard of polystyrene pyrolyis to produce styrene, would any other plastic make medium chain alkanes? Here's a very long thread on the subject which I haven't read all the way: http://www.energeticforum.com/renewable-energy/7040-how-turn... he claims 17 cents a liter which seems too low to me.

http://www.sciencemadness.org/talk/viewthread.php?tid=24683#... This thread touched on the subject but most of the discussion centered around PVC for some reason. I'm more interested in polyethylene as various forms are very common in commercial and residential waste streams.

I've attached two PDFs of interest, one shows that pyrolysis products from "assorted plastics" yielded a product comparable to diesel and ran in an unmodified engine. Unfortunately an unspecified catalyst was used and the plastic composition is a mystery. The other paper shows medium chain parafins were produced by thermal decomposition of HDPE without catalyst.

What do you guys think? I'm not in a position to start distilling lots of waste plastic but you could imagine if you could run the product in an unmodified diesel engine you could get lots of waste plastic for free and if you had solar or wind on your property use that to distill the plastic and potentially generate your own fuel or store your energy in liquid form.


Attachment: Pyrolysis of HDPE in a diesel engine.pdf (777kB)
This file has been downloaded 1161 times

Attachment: Pyrolysis of polyethylene.pdf (2.6MB)
This file has been downloaded 1389 times


j_sum1 - 11-6-2015 at 18:52

I think it is something that should be done more often. There is so much energy locked up in waste plastic, to throw it away is nearly criminal and that s before we start talking about the environmental detriments of said plastics.

As for the specifics of your question, I believe the issue that comes up most often with repurposing plastic products is the huge mixture of chemicals that arise both from the main polymer and also from additives and contaminants. This complexifies any processes and leads to a lot of unknowns in your product stream. In the case of diesel fuel, you really want some assurance that your product is going to be non-polluting as a fuel. (Or at least no worse than diesel already is.) That is a difficult thing to guarantee.

On the other hand, if you devise/adapt a method that is practical then you are onto a sure winner here.

phlogiston - 12-6-2015 at 00:55

Isn't plastic waste already being incinerated and the heat commonly used for electricity production?

If your goal is environmental, you should also consider the gasses and soot vented during pyrolysis and the possible additional emissions from the car running on this fuel.

It seems likely to me that thorough incineration in a plant built fot that purpose and of which the emmissions are properly monitored will perform better overall.

froot - 12-6-2015 at 01:39

De-polymerising plastic is your goal and pyrolysis is one way to do it although it is energy intensive and your product will be random. It 'boils' down to how much energy you throw at the process vs the energy in your product before you even start considering the quality of your product.
Find an efficient way to crack a polyethylene chain for example at predetermined points of the polymer to either produce fuel or recycled feedstock to the plastic industry and you'll be on the road to riches.

blogfast25 - 12-6-2015 at 07:02

Quote: Originally posted by crazyboy  

This got me interested, I have heard of polystyrene pyrolyis to produce styrene, would any other plastic make medium chain alkanes? Here's a very long thread on the subject which I haven't read all the way: http://www.energeticforum.com/renewable-energy/7040-how-turn... he claims 17 cents a liter which seems too low to me.



I must say I'm amazed at the degree of depolymerisation obtained in 4 h @ 350 C and w/o any catalyst used at all.

The energy cost works out at about 8 pence/kg of product, very roughly:

1 kWh = £0.10

6 kW x 4 h = 24 kWh = £2.4 for 30 kg (single reactor pass end-product)

So 8 p/kg (twice that for a two pass product, obviously)

Factor in some 'economy of scale' for much larger depolymerisers, residual heat recovery from the hot, finished product and a decent but cheap catalyst and the possibilities seem endless.

Something just sounds too good to be true but ra ra, what is it? :o

And of course it's a fossil fuel 'in disguise'...


[Edited on 12-6-2015 by blogfast25]

Dr.Bob - 12-6-2015 at 10:18

For plastics that are not easily recyclable, it would make more sense to me to just have more municipal incinerators with heat recovery electric generators and scrubbers, and burn all of the non-recyclable trash. Burying it is stupid, and burning it will provide ash that is high is some minerals, so it might even be profitable to use it as feedstock one day. But Pyrolysis could generate some power, I have seen an actual pilot plant system for this, but it is not nearly as easy or profitable as claimed. The energy input is large to start and then tapers off if you have good energy recovery systems, but the output is far less that expected, as there is a large amount of moisture in most trash streams, and the system has to remove that as steam, which removes a lot of energy from the system. My understanding is that for every 2000 pounds of trash/waste, it can generate about 50 gallons of crude fuel, which is not good enough for running an engine without further purification and other treatments (hydrotreating?) to get the fuel either more like diesel or gasoline, as both have tight specs. But the system cost over a million to build (government grant pricing, however), and can only produce a 100 gallons per day right now. So you would need to get the capital price down a lot and the throughput up to make it practical. Plus even for garbage, you need someone to haul it to you, a place to store it, and about 100 government permits to operate the system.

crazyboy - 12-6-2015 at 16:20

Quote: Originally posted by froot  
De-polymerising plastic is your goal and pyrolysis is one way to do it although it is energy intensive and your product will be random. It 'boils' down to how much energy you throw at the process vs the energy in your product before you even start considering the quality of your product.
Find an efficient way to crack a polyethylene chain for example at predetermined points of the polymer to either produce fuel or recycled feedstock to the plastic industry and you'll be on the road to riches.


Thermal decomposition isn't very energy intensive, as shown by the guy who was able to produce the hydrocarbon mix for 17 cents per liter. Why would you need to crack it at a predetermined point? Diesel is a mix of various chain lengths and thermal decomp results in mostly C9-C20 chains which is basically what diesel is.

Quote:

My understanding is that for every 2000 pounds of trash/waste, it can generate about 50 gallons of crude fuel, which is not good enough for running an engine without further purification and other treatments


50 gallons per 2000 pounds translates to 0.2 liters per kilogram. The guy from the energetics forum claimed he was getting 1L/kilo. The first paper I posted indicates that the products are effectively a drop in replacement for diesel. Additionally on the second page of that forum post the guy says he bought 1 ton of shredded plastic from a recycling place for $50. 2000Lbs is about 900Kg if he gets about 1L/Kg that's 900L of fuel or 230 gallons.

Might not be right for the guy living in suburbia but could be very appealing to someone living off the grid, gas or diesel doesn't have an infinite shelf life, only a a year or two if I recall. Plastic does and if you could buy it at $50 a ton you could store it in a silo and generate diesel for your truck or generator from solar as you go. The only issue I see is the potential environmental cost, but if you can dispose of the ash safely than its really no worse than buying diesel from the gas station.

[Edited on 13-6-2015 by crazyboy]

phlogiston - 13-6-2015 at 07:22

The main problem with long term storage of gas and diesel is that the most volatile components evaporate. If you can obtain a sufficiently well sealed container, it should be possible to store it pretty much indefinitely.

blogfast25 - 13-6-2015 at 08:19

Quote: Originally posted by crazyboy  

50 gallons per 2000 pounds translates to 0.2 liters per kilogram. The guy from the energetics forum claimed he was getting 1L/kilo. The first paper I posted indicates that the products are effectively a drop in replacement for diesel. Additionally on the second page of that forum post the guy says he bought 1 ton of shredded plastic from a recycling place for $50. 2000Lbs is about 900Kg if he gets about 1L/Kg that's 900L of fuel or 230 gallons.



The 1 L/kg number is of course much closer to the 0.2 one. What goes in must come out and at 0.2 L/kg that would require a very high (and unrealistic) degree of depolymerisation to 80 % gases (C < 4, basically).

I think if you're going to put depolymerised plastic into your car tank, you'll have to pay tax on it, which is a great disincentive for most people. Use as home-heating diesel?

Dr.Bob - 14-6-2015 at 19:14

The number I posted was for a mixed trash system, so likely much less usable material, plus water, glass, etc, thus the low recovery. But since most plastic is much less then 1 kg/1L in density, I think it would be very hard to generate any real recovery near 1 kg/ L, as the mix of material recovered will include gases, liquid and ash, so the usable fuel would be more likely to be about 500 g per 1L at best in the real world.

You can put nearly any fuel in your vehicle, but if you burn anything that is not ASTM certified (what you buy at the gas station) then your engine warranty is voided. And many fuels from pyrolysis could contain things that might not be ideal for an engine. Just like you can burn straight veggie oil in a diesel engine, but it will ash up quickly and be destroyed eventually. But burning quality biodiesel at 5-85% in regular diesel will not damage most diesels. Don't believe everything people claim on the internet or even in papers. I don't think the author of a paper will warranty your engine...

And while most alternative fuels are taxed when sold, and the law requires it, you could likely add a little alternative fuel to your tank every so often and not get caught. I have known several people to add waste MTBE, iso-octane, benzene, toluene, methanol, ethanol, etc to their gas tank in small amounts, and it is fine if done in small amounts. Just don't use n-alkanes such as n-octane or n-hexane, as that will lower your octane rating badly and kill your engine.

Cloner - 19-6-2015 at 02:01

I heated some waste PE in a test tube over an oxidizing bunsen flame, for 5 minutes. About 20% of low MW combustible gases evolved.

The residue is a brittle wax which smells of hydrocarbon. Clearly, oligomers have formed.

In a separate experiment, petroleum was heated to a low reflux onto small amount of iron sponge (also heated with oxidizing bunsen flame)in a test tube. There is a continuous evolution of alkenes, but this is a very slow process. The wax from the earlier experiment does not generate appreciable amounts of alkene in this setup, because of it not refluxing.

aga - 19-6-2015 at 12:11

When i tried PVC pyrolysis, 260C was when the action happened (decomposition gasses started coming out).

kecskesajt - 20-6-2015 at 09:11

Quote: Originally posted by Cloner  
I heated some waste PE in a test tube over an oxidizing bunsen flame, for 5 minutes. About 20% of low MW combustible gases evolved.

The residue is a brittle wax which smells of hydrocarbon. Clearly, oligomers have formed.

In a separate experiment, petroleum was heated to a low reflux onto small amount of iron sponge (also heated with oxidizing bunsen flame)in a test tube. There is a continuous evolution of alkenes, but this is a very slow process. The wax from the earlier experiment does not generate appreciable amounts of alkene in this setup, because of it not refluxing.

Look at this video.The person is using clay pot pieces.It might be faster
http://youtube.com/watch?v=7M7RY04KKBs

blogfast25 - 20-6-2015 at 10:05

Quote: Originally posted by aga  
When i tried PVC pyrolysis, 260C was when the action happened (decomposition gasses started coming out).


I really think you should continue those experiments, using test tubes ('boiling tubes') and a more 'quantitative' set up. A Bunsen should provide ample heat to get to a high degree of depolymerisation. A train of simple wash bottles/condensers culminating in a simple gazometer should provide ample useful information re. HCl generated and gaseous and liquifiable decomposition products.

blogfast25 - 20-6-2015 at 10:15

Quote: Originally posted by kecskesajt  

Look at this video.The person is using clay pot pieces.It might be faster
http://youtube.com/watch?v=7M7RY04KKBs


Nice find.

Tip for future experimenters: wrapping ordinary (NR or SBR based) rubber stoppers in teflon tape ('gas tape') can protect them quite adequately from high heat/corrosive gases (HCl e.g., in the case of halogenated polymers)

kecskesajt - 20-6-2015 at 11:40

Wow my father have a dozen of PTFE tape.And OMG,Im burned some tape inside the house :O.I noticed how shitty smell it has.

xfusion44 - 25-6-2015 at 04:06

I thought it'd be helpful if I'd post some pictures of my plastic pyrolysis apparatus design for those of you, who are just starting with pyrolysis of plastic ;)


Remove the threaded plastic piece:

2014-08-04.jpg - 51kB

2014-08-05.jpg - 31kB

IMG_20140805_023107.jpg - 985kB

IMG_20140805_023123.jpg - 1.1MB

IMG_20140805_023146.jpg - 1MB

On the end of copper tube where it's attached, there is round piece of copper sheet soldered on and gaps are sealed by PTFE tape.

End product:

IMG_20140806_004035.jpg - 1.3MB IMG_20140806_004101.jpg - 1.1MB

Not all plastic was consumed in making those 50 ml's of product, it was just a test run.

PS: procedure: throw pieces of plastic into the can, close it and place bunsen burner underneath it, dip the end of the tube into beaker/container with cold water and wait for your product to collect on the water's surface. (hot plate can't be used, since it can't reach plastic's boiling point), also you may need to replace or let water cool down every once in a while, since it heats up due to hot plastic pyrolyis product that condenses in it which may result in boiling water splattering your product all over the place and/or loss of product due to insufficient cooling and excessive evaporation.

BR, xfusion

[Edited on 25-6-2015 by xfusion44]

[Edited on 25-6-2015 by xfusion44]

blogfast25 - 25-6-2015 at 05:23

Be careful heating cans that aren't designed for that, with flammable liquids forming inside! :o:o

Also, create a little copper coil and run it through running water, to act as a more efficient condenser.

An anti-suckback valve is also to be recommended, to avoid violent steam explosions in case of suck back.

A mass balance would also have made it more scientific: how much plastic did you start from, how much residue did you end up with and how much liquid product?

[Edited on 25-6-2015 by blogfast25]

xfusion44 - 26-6-2015 at 06:34

Quote: Originally posted by blogfast25  
Be careful heating cans that aren't designed for that, with flammable liquids forming inside! :o:o

Also, create a little copper coil and run it through running water, to act as a more efficient condenser.

An anti-suckback valve is also to be recommended, to avoid violent steam explosions in case of suck back.

A mass balance would also have made it more scientific: how much plastic did you start from, how much residue did you end up with and how much liquid product?

[Edited on 25-6-2015 by blogfast25]


Product is not very flammable, don't worry ;) It's not even so easy to ignite it directly with lighter.

I tried to avoid suck back with removing tube from water before turning off the flame, but it did happen to me, when I ran out of gas :) It wasn't so violent as the mass of plastic inside is not big and also walls of the can are thin, so they can cool down really fast. (I don't even remember steam coming from the tube) But yeah, valve would be recommended (in this case implosion could happen).

I thought about the coil running through water, but I didn't have enough pipe. If I'd do it this way, I could even avoid using suck back valve.

I know it would be a lot better to write down how much plastic I've used and how much product I've got, but at the time I was just wondering if this would make a good fuel and unfortunately I didn't weigh the plastic, but I'd say that about 1g of plastic is enough to make 1ml of product, so maybe about 50 grams for the quantity on picture (just my guess). Somewhere I also saw, that 1kg of plastic is enough to make 1l of fuel, so that would be possible I think. Depends on the type of plastic too, I'd say.

Thanks for all of the safety tips :)

xfusion

aga - 26-6-2015 at 08:00

Quote: Originally posted by xfusion44  
throw pieces of plastic into the can

Did you use all one type of plastic or a mixture ?

This may help identification :-
http://www.garrison.hawaii.army.mil/sustainability/images/Pl...

blogfast25 - 26-6-2015 at 08:32

Quote: Originally posted by aga  

http://www.garrison.hawaii.army.mil/sustainability/images/Pl...


Incidentally, polyprop should be slightly easier to depolymerise (than PE) due to the tertiary carbon in its structure.

Dr.Bob - 26-6-2015 at 12:43

Yes, knowing the plastic used is key, as each plastic is likely to provide a different liquid upon heating, some of which would be better then others for fuel. For example, Acrylic is easy to depolymerize into methyl methacrylate, but if you put it into your gas tank, it would eventually re-polyumerize, and that might not be good for your fuel pump. I would think that polystyrene would be practical, but again, styene can polymerize, so in practice, most industrial pyrolysis systems hydrogenate the fuel to remove unsaturated bonds, as they can be problems if activated towards polymerization. Unsaturated bonds do tend to make the fuel more liquid that the equivalent saturated hydrocarbon (lower MP), which can be useful for diesels to prevent gelling (freezing) in the winter.

aga - 26-6-2015 at 12:53

PVC goes to loads of HCl and foul smelling carbon.

Tried that with a few 100g PVC.

xfusion44 - 26-6-2015 at 13:23

Quote: Originally posted by aga  
Quote: Originally posted by xfusion44  
throw pieces of plastic into the can

Did you use all one type of plastic or a mixture ?

This may help identification :-
http://www.garrison.hawaii.army.mil/sustainability/images/Pl...


At first I wanted to use one type... But then I ended up with mixture (mostly PS and PE). I think I'll try with only one type when I'll have some time too, because I'm interested to see different colors, flammabilities and other properties when using certain plastic :)

xfusion

aga - 26-6-2015 at 14:43

dear xfusion44.

I love your enthusiasm to try stuff out, and applaud your making of a Pyrolysis rig out of scrap stuff, and especially for Doing It.

It is Wonderful, Exciting, Fun and really Good to see Stuff happen.

It isn't Science though is it ?

'Science' is your Next Step, where you present Evidence, and not just What You Did.

Get only 1 kind of Plastic, weigh it as best you can.
(ebay: 0.01g scales are dirt cheap)

Pyrolyse it, and measure, and write down everything you can : temperature(s), time, what you see, what you smell - everything !

e.g. weigh the water & collection vessel before & after. The difference is how much stuff you got. If you see smokey stuff coming out of the collection vessel, note the time, temperature and what it looks like, what colour it is.

Do it like that and many people here can analyse and work out stuff from what You Did that neither you nor i could dream of (yet).

[Edited on 26-6-2015 by aga]

xfusion44 - 27-6-2015 at 12:08

Quote: Originally posted by aga  
dear xfusion44.

I love your enthusiasm to try stuff out, and applaud your making of a Pyrolysis rig out of scrap stuff, and especially for Doing It.

It is Wonderful, Exciting, Fun and really Good to see Stuff happen.

It isn't Science though is it ?

'Science' is your Next Step, where you present Evidence, and not just What You Did.

Get only 1 kind of Plastic, weigh it as best you can.
(ebay: 0.01g scales are dirt cheap)

Pyrolyse it, and measure, and write down everything you can : temperature(s), time, what you see, what you smell - everything !

e.g. weigh the water & collection vessel before & after. The difference is how much stuff you got. If you see smokey stuff coming out of the collection vessel, note the time, temperature and what it looks like, what colour it is.

Do it like that and many people here can analyse and work out stuff from what You Did that neither you nor i could dream of (yet).

[Edited on 26-6-2015 by aga]


I totally agree, but at the time as I said, I just wanted to see if some useful fuel could be made and I didn't bother weighing and analysing product and materials used.

When I'll try it next time I'm sure I'll document everything. I'll test only one plastic at once, take pictures, write down all weight data, color, smell...

I bought one of those scales long time ago on ebay, but it didn't last (worked only for 5min and then didn't want to turn on, now it turns on only if you let it sit untouched for long time and even then only for half minute).

BR, xfusion

aga - 27-6-2015 at 13:27

I tend to want to 'just do it' as well.

Experience has shown me that by NOT measuring stuff and writing stuff down, i get Lucky one time, and cannot reproduce the same result ever ever again !

Maybe a camera/voice recorder would be better.

blogfast25 - 27-6-2015 at 13:51

aga:

Trying to promote the Scientific Method<sup>TM</sup> on an 'amateur science' forum, huh? We'll have none of that newfandangled nonsense here, Sir! Next someone will claim pure substances contain 'chemical elements' (and not earth, wind and fire... and phlogiston...) in fixed ratios! They chopped that rebel Antoine Lavoisier's<sup>*</sup> head off for that. Halcyon days!

More of this behaviour from you Sir and I will have to pick up my finest quill and lodge a formal complaint with the Honourable President of our Society.

<sup>*</sup> Oh, no, wait... it was because he was a tax collector!


[Edited on 27-6-2015 by blogfast25]

aga - 27-6-2015 at 14:04

Reported.

You just had to go and say the T word.

cracking of plastic

CrossxD - 8-7-2015 at 11:31

I found this topic:
http://www.sciencemadness.org/talk/viewthread.php?tid=62720
Is there another possible way to crack plastic? for example using catalyst?

aga - 8-7-2015 at 11:58

Heat is a cheap and easy to obtain catalyst.

Others things might work.
Try some things and see.e.g. Al powder.

Zombie - 8-7-2015 at 13:44

Toluene is an excellent solvent of plastics. I'm sure you could dissolve a polystyrene/styrene, ABS, ect... into a liquid, and separate the components from there.

Benzine, and Xylene may work for you as well.

aga - 8-7-2015 at 13:55

I think the OP is looking for a way to decompose the polymer into it's bits rather than dissolve it.

Hard to tell.

Very random and non-specifiec question really.

e.g. Which plastic ? What kind of cracking ?

Could be just making a crack in some random plastic, or a question about how to make crack cocaine out of a random plastic, or a physics question about how to crack the equation that could predict the polymerisation sequence.

Personally i have no idea which with the data supplied.

Zombie - 8-7-2015 at 19:27

Oh... To make crack you need a fry pan, some road flares, baby aspirin, and three cups of GOOD quality English tea.
Either the baby aspirin or the tea contain crack. Babies and brits are soooo messed up. It's hard to know which has it.

Seriously,I thought you meant separation thru distillation (cracking) of some random plastic. Liquefying it would seem a logical step.

kecskesajt - 14-7-2015 at 23:40

It is nice but what if some halo-carbons get into it and makes the exhaust fumes corrosive and possibly make phosgene.And can the oil polymerise into the tubing?
SFMBE