Sciencemadness Discussion Board

Making Lithium Metal

BromicAcid - 6-5-2004 at 17:17

I found it odd that in my quest to find a reliable procedure for the procurement of sodium metal from its commonly available salts I would stumble more often then not over detailed procedures for the production of lithium in the lab setting instead. Now, not wanting to be wasteful in my hording of information I present the culmination of the methods that I have run across. People are welcome to elaborate on any given technique, criticize its effectiveness, or even add their own, this is the lithium production thread, but hopefully I will be comprehensive enough during this initial stage as to prevent it from growing to the size of the sodium thread.

Molten Salt Electrolysis


(From Complete Treatise on Inorganic Chemistry)
Quote:
In R. Bunsen's apparatus, an iron wire and graphite rod dip into the fused chloride without the aid of the clay pipe. In a few seconds, says Bunsen, a small silver-white regulus is formed under the fused chloride round the iron wire, and adhering to it, which, after 2 or 3 minutes, attains the size of a small pea. To obtain the metal, the wire pole and regulus are lifted out of the fused mass by a small, flat, spoon-shaped iron spatula. The wire can then be withdrawn from the still molten metal, which is protected from ignition by the lithium chloride with which it is still coated. The metal, after cooling under rock oil, may now be easily taken off the spatula with a pen-knife. As this operation can be repeated every three minutes, an ounce of lithium chloride can be reduced in a very short time. In F. Hiller's modification, lithium chloride, mixed with ammonium chloride, is heated to its m.p. in a porcelain crucible, See above figure. A piece of iron wire, passing though the bore of a clay tobacco pipe inverted in the molten chloride serves as the cathode; and a rod of retort carbon serves as anode. For the sake of clearness, the drawing, has been made as if the parts of the apparatus were transparent. If desired a stream of dry hydrogen gas can be passed into the tobacco pipe so that the liquid about the cathode is not exposed to oxygen. A current from a battery giving 7 to 8 volts serves for the electrolysis of the molten chloride. The reduced lithium rises to the surface of the liquid in the compartment where it is protected from oxidation. Before using the apparatus it is advisable to cover the crucible and pipe in a layer of powdered graphite made into a slip with a dilute solution of lithium chloride. The coating is dried and baked at red heat. This prevents the formation of lithium silicide by the action of the fused chloride on the clay. After an hours electrolysis, the apparatus can be cooled, and the regulus of lithium can be removed by breaking the pipe.


(From Preparative Inorganic Chemistry)
Quote:
Electrolytic Preparation of Lithium
LiBr ---> Li + 1/2 Br
Pure Li is prepared (via the method of Ruff and Johannsen) from LiBr which is melted in an electric arc in the presence of 10 - 15% LiCl (the LiBr is obtained from Li2CO3 by evaporating the latter from hydrobromic acid). The figure is a scale drawing (1:5 [Hence my inclusion of a ruler]) of the Muthmann electrolysis vessel used for the melting procedure. It is made of copper and its upper part is cooled with water. While the melting point of pure LiBr is about 546C and that of LiCl is 606C, a mixture of LiBr with 15% LiCl solidifies at 520C. The electrolysis proceeds at 10v. (as measured across the terminals) and 100 amp. A graphite rod is used as an anode and two 4-mm. iron wires serve as cathodes. The metal which deposits at the cathodes, is scooped up from time to time with a flat iron spoon and, while still liquid, is separated from the solidified melt on a cold stone plate. It is next freed of adhering salt using Brochers' method, i.e., by immersion in a paraffin bath (180 - 200C). The salt settles to the bottom, while the metal rises to the surface. After cooling, it is washed with ligroin. It is stored under ligroin (d. 0.56) in completely filled, tightly closed vessels.

Different Melts for electrolysis:
LiCl 52.9 mol% Li2CO3 19.8 mol% Li2SO4 27.2 mol% MP 445C Yield not stated
LiCl 75 mol % Li2CO3 25 mol % MP 507C Yield not stated
LiCl 50 mol % KCl 50 mol % MP 404C Yield not stated (Makes technical grade Li)
Quote:
From Comprehensive Inorganic Chemistry
Fused LiCl and KCl is electrolyzed in a cell containing a graphite anode and a mild steel cathode. The electrolyte is maintained at 404C, and the voltage at 5.2, and the current density at 3.53 amp/sq in.

LiBr w/ 10 - 15% LiCl MP 520C Yield 80%
Electrolysis in Non-Aqueous Mediums

From Complete Treatise on Inorganic Chemistry:
Quote:
Lithium cannot be obtained by the electrolysis of aq. soln. of its salts, but L. Kahlenberg obtained it by the electrolysis of soln. of the chloride (Reference 1) in pyridine, acetone, or in various alcohols. Silvery white lithium obtained from a conc. soln. of lithium chloride in pyridine at the room temp. using a graphite plate as anode, and an iron plate as cathode with 0.2 to 0.3 amp. per 100 sq. cm. of cathode surface, and a potential difference of 14 volts.
(Reference 1) S. von Laszczynsky, Organische Flussigkeiten als Losungsmittel fur anorganische Saltz, Berlin, 1894 ; Ber., 27. 2285, 1894 ; Zeit. Elektrochem., 2. 55, 1895 ; S. von Laszczynsky and St. von Gorsky, ib., 4. 290, 1898 ; L. Kahlenberg, Journ. Phys. Chem., 3. 601, 1899 ; H. C. Patten and W. R. Mott, ib., 8. 153, 1904

From Comprehensive Inorganic Chemistry:
Quote:
For example, the alkali chloride or bromide is fused with aluminum chloride or bromide and the fused mass is dissolved in nitrobenzene and electrolyzed. By this method, lithium, sodium, potassium, and rubidium can be deposited on the cathode. The alkali ion serves as the cation, and the aluminum appears in the complex anion.

However, to my knowledge alkali metals produced in this way are impure. Also explosions can result and the yields are low. Additionally Li can be produced from a solution of LiCl in liquid ammonia or hydrazine.
Purely Chemical Methods

Reduction of LiOH or Li2CO3 or LiCl with magnesium as stated in Complete Treatise on Inorganic Chemistry is explosive but 40% magnesium oxide can be added to moderate the reaction. Information relating to chemical reduction by Mg or Al can be found if you see Warren, Chem. News, 1896, 74, 6, and U.S.P. 2028390. Lithium salts such as LiNO3, Li2CO3, and LiOH can be reduced with carbon or metal carbides or even calcium at high temperatures. Zirconium is an effective reducing agent for nearly any alkali metal that is combined with oxygen, it will reduce sulfates and phosphates in a self sustained reaction.
From Comprehensive Inorganic Chemistry:
Quote:
For example, iron displaces the alkali metal sulfates and arsenates at their melting point, from thiocyanates at 650C, from borates and phosphates at 1300-1400C.... Alkali metal compounds such as hexacyanoferrates(II), cyanides, and azides can be decomposed into the alkali metal by heating.

However the Complete Treatise on Inorganic Chemistry states the lithium cannot be prepared by the reduction of lithium compounds with iron.
Other interesting things dealing with Lithium

From Descriptive Inorganic Chemistry 3rd edition, Geoff Rayner-Canham; Tina Overton:
Quote:
Liquid lithium is the most corrosive material known. For example, if a sample of lithium is melted in a glass container, it reacts spontaneously with the glass to produce a hole in the container, the reaction being accompanied by the emission of an intense, greenish white light.

Lithium vapor is red!

Finally, an overview of the physical properties of lithium taken from here.

Atomic number 3
Atomic mass 6.941 g.mol -1
Electronegativity according to Pauling 1.0
Density 0.53 g.cm -3 at 20 °C
Melting point 180.5 °C
Boiling point 1342 °C
Vanderwaals radius 1.55 nm
Ionic radius 0.06 nm
Isotopes 2
Electronic shell 1s22s1 or [He] 2s1
Energy of first ionisation 520.1 kJ.mol -1
Standard potential - 3.02 V
Discovered Johann Arfvedson 1817

Note, lithium compounds are neuro toxins.

blip - 8-5-2004 at 12:50

Just a few days ago I extracted a few slivers of Li from Energizer e<sup>2</sup> Li batteries that I got for $18. Really I only started extraction on one of the 8 batteries in the pack, supposedly giving me .94 g Li for $2.25 though I only have one reference to the supposed amount. At another store the day before I began, I got great deals on butane lighters and mineral oil, the latter which without I could not store the Li or even begin to halt any highly energetic reactions inside the open battery. I read up on <a href="http://www.rhodium.ws/">Rhodium's site</a> about it much before and felt that I have no other easy source of an alkali metal, especially one that does not easily form peroxides or superoxides. I strongly encourage anyone attempting this to try to do it all under mineral oil or whatever you plan to use, because what I think is MnO<sub>2</sub> can be squeezed into more contact with the Li causing a reaction that could go out of control if you simply try to keep the open segment "wet". The worst that has happenned under the oil bath was a red glolwing spark that went out, though prompting me to stop for the day. In the air remaining "wet", twice it smoked with the first occurence glowing and that's when I dunked it into a container full of oil for that purpose. Apparently, there was a piece of metal that I tugged on that initiated the reaction and only came out "safely" completely under the oil.

I first removed the label, then successively cut near the anode two lines ~45&deg; apart so that I could use pliers to peel. I monitored the temperature and paid special attention to make sure that I didn't cut past the metal, which seems almost impossible. This killed the blade :( so don't use your best one; perhaps you may have another method that is superior. I freaked multiple times when when the battery warmed--due to me body heat and tight grip, combined with my tension! You may find a strip, one I found was apparently Li but according to a reference there is another that isn't Li. Additionally, there are layers of Li and MnO<sub>2</sub> in the large plastic roll. I used my pocket knife's scissors to cut through each layer of plastic after I had got the Li on it. I do not know if one could cut open the entire battery and unroll the plastic film and then get a large layer of Li, but I may try it when I next need Li for something (no use yet, so I expect it to be a LONG while considering my fright). Oh yeah, get used to all of the black (supposedly red-brown) nitride that'll be all around when you're done.

BromicAcid - 8-5-2004 at 13:37

For me I got lithium from taking apart military grade batteries from eBay. I got a Lithium/Sulfur dioxide battery for $2.99, it was about the size of a lantern battery. I carefully took it apart and it was segmented into 8 smaller batteries.

So experimentally I drilled a hole into one of them and lo and behold like I wasn't expecting it, sulfur dioxide sprayed out as a mist. The liquid bubbled out from the hole and the air was thick with it. So I took the battery and tossed it into some NaOH solution I quickly made up, the SO2 was completely absorbed before bubbles broke the surface. After it stopped that I took a hack saw and cut around the battery and broke it in two. It had a large wad in the middle of two different materials in rolls wound around one another.

Pulling the two of them apart I found that one was blackened and the other gray. I took a piece of the one and tossed it in water with no reaction. The other though gave a definite indication that it was lithium, skittering around the surface and bubbling furiously. I quickly weighed the lithium, 5 g and balled it up and put it in mineral oil, after dunking it up and down several times it took on enough oil to make it more or less static in its movement and pushed it to the bottom. And that is my story of extracting lithium metal from batteries.

However I really have no use for it, still doesn't mean I don't want to stock pile it. Going for electrolysis of the chloride in a week or so, using a 1 1/2 inch copper endcap for pipe as my vessel. Bent some glass tubing around the top for cooling, easy to obtain the iron wire and the graphite anode was also easily obtained.

Lithium from Pyridine

Strepta - 15-5-2004 at 17:05

posted by BromicAcid

[Lithium cannot be obtained by the electrolysis of aq. soln. of its salts, but L. Kahlenberg obtained it by the electrolysis of soln. of the chloride (Reference 1) in pyridine, acetone, or in various alcohols. Silvery white lithium obtained from a conc. soln. of lithium chloride in pyridine at the room temp. using a graphite plate as anode, and an iron plate as cathode with 0.2 to 0.3 amp. per 100 sq. cm. of cathode surface, and a potential difference of 14 volts. ]


Last December I thought I'd try the electrolysis of LiCl in pyridine, so I purchased 500ml of pyridine for $60 (ouch!!) I used a graphite anode and a nickel cathode (approx. 2 sq. in.) Spacing between electrodes was about .75 in. I was able to dissolve 2 g of LiCl in 30 ml of pyridine. Applying voltage, I could hardly detect any current flowing. For 30v across the electrodes there was perhaps 15ma of current. The LiCl must not be ionized. Doing a little math after the fact, it takes about 100,000 coulombs to reduce a mole (7 grams) of Li+ ions to Li. At .015A that would take about 2000 hours or much larger plates and I have better things to do. Also, pyridine is not all that pleasant to have around as it smells a lot like skunk. Live and learn I guess.

J Phys Chem

S.C. Wack - 15-5-2004 at 17:51

I read his articles (there are later ones in that journal) and thought that there may be some cottage-industryness to it if there was enough demand and cheap electricity. But if I remember correctly, it is a very touchy procedure, for several reasons. The pyridine must be very dry, and stay that way. He did not get good results with the other solvents, either. Would take some work, and this would probably not be a side project, but something you would devote a lot of effort towards, like Kahlenberg did.

vulture - 16-5-2004 at 07:59

How about DMF or DMSO?

DMSO is pretty readily available in the states I hear.

BromicAcid - 16-5-2004 at 09:14

Currently warming my frozen bottle of DMSO up under my arm pit. If the weather holds I will get back to this in a bit. Burrrr...

The solubility of lithium compounds and analogous sodium compounds (but we all know how lithium compounds differ from the other alkali metals on some things) have persuaded me to give this a shot. As well as the lack of reactivity of Na in DMSO until a high temperature and that DMSO is an ionizing solvent. Too bad I don't think my DMSO is anhydrous, might have to dry over Na wire first.

Edit 1: Got too cold holding the DMSO in every crevasse of my body so I put it in a pan of hot water to heat up. Went out back and found out that I was out of LiCl :( so I had to neutralize some carbonate with HCl so this is going to take awhile, stupid hygroscopic/disquecent LiCl, it's boiling away right now though.

Edit 2: Gahhhh DMSO dripped on the side of the bottle or something and it got on my skin, stupid 99% DMSO, it leaves the most rank aftertaste I can describe and it just enters your body where it pleases.... Grrrr...

Edit 3: LiCl dry and commencing electrolysis, notice my axehandle style editing today ;)

[Edited on 5/16/2004 by BromicAcid]

[Edited on 5/16/2004 by BromicAcid]

[Edited on 5/16/2004 by BromicAcid]

Very Interesting...

BromicAcid - 16-5-2004 at 13:20

My write-up as play by play style:

20ml of DMSO was placed in a small test tube and 1 chunk of LiCl of approximately 1.2 g was added to the DMSO. The piece was crushed with the aid of a stirring rod and a powder remained at the bottom of the test tube. It should be noted that my DMSO was 99% and was not subject to additional purification and that my LiCl although freshly dried from solution probably still contained a percentage of H2O along with metal ions present in the OTC HCl used in its preparation.

A nickel anode and cathode were placed into the solution and electrolysis was begun at 6V. Immediately bubbles began to form at the cathode and the after a few moments the anode started to take on a blue hue that gradually began to settle to the bottom forming some nickel salt, NiCl2 probably.

A further minute or two passed and the cathode started to turn black and a red/brown/black cloud started to plume up from it to the surface. The solution began to gradually darken but the red color still stuck largely to the top and continued to rise from the cathode as nickel salts continued to descend and cover the very bottom of the test tube.

A very strange smell started to come from the solution, not unlike rotting eggs but entirely different from H2S. By this time the voltage had be raised to 12V with the visual clue being the increase in evolution of bubbles and red liquid from the cathode. The red liquid had a distinct top layer at this time but it could have just been the meniscus of the test tube refracting the color oddly.

After about 8 minutes from the commencement of electrolysis the application of electron movement to the solution was discontinued. Still LiCl remained undissolved at the bottom and there was a color of Ni salt at the bottom in solution. The red color was at the top and the electrodes were removed from the solution, I noticed by this time a somewhat intense garlic/onion smell.

The anode electrode was somewhat clean and shiny but slightly pitted. At the very end LiCl was stuck to it coated in nickel salts turning it blue. The cathode was black with nasty looking flecks and chunks covering it. It had an unusual smell even different then the solution that escapes my descriptive capabilities. As I inspected it, it started to fume in the air. My heart almost skipped a beat, I spit onto my work bench and rolled the electrode in it (My surefire test for alkali metals, although not 100% reliable, the reagents are readily avalible ;)), and it started sizzling and boiling on the surface, lithium metal had been achieved as a non-adherent black coating. Holding the test tube up to the sun I noticed flecks throughout the solution, "Lithium?" I thought to myself.

I added a bit of H2O to the test tube, only a tiny bit and the darkness immediately began to dissipate in a disproportionate manner to the water I added, much more so then could be accounted for by dilution. A few of the black shavings in the solution bubbled away but most stayed suspended unaffected.

I rinsed out the testube with water and got even more weird smells. The anode washed clean instantly but the cathode had an adherent coating on most of it that would hardly scrape off, NiO?

Regardless, it was an interesting experiment, thank you Vulture for your idea! My guess is that the lithium being generated at the cathode was just reducing the DMSO. In the end the solution was luke warm, to be expected from the heat of electrolysis. Lots of pretty colors though. :D

Edit: Looked up the Rxn. between alkali metals and DMSO, supposedly sodium and potassium react with DMSO by cleaving the carbon-sulfur bond:

CH3SOCH3 + 2Na ---> CH3SONa + CH3Na
CH3SOCH3 + CH3Na ---> CH3SOCH2Na + CH4

"Electrolytic reduction of NaCl or NaI in DMSO similarly leads to a mixture of hydrogen and methane gasses at the anode." Funny thing is I only got gas evolution at the cathode....

[Edited on 5/16/2004 by BromicAcid]

BromicAcid - 17-5-2004 at 18:56

I've been trying to figure out all the reactions that were occuring during my electrolysis of LiCl in DMSO. My anode reaction seems straightforeward:

Ni(s) ---> Ni2+ + 2e-

The charge being balanced by the chlorine anions still in solution.

However my cathode reaction is a bit more complex. I would like to think that the only thing occuring would be:

Li+ + e- ---> Li(s)

However with all the colors and bubbling that occured there was a bit more to it.

Sure, the lithium may have depositied and almost instantly reacted away but what was the end product.

My cathode was covered in a black adherent coating, NiS, NiO, C ? I need to do more tests. The bubbles generated could have been CH4 as supplied by my above set of equations:

CH3SOCH3 + 2Li ---> CH3SOLi + CH3Li
CH3SOCH3 + CH3Li ---> CH3SOCH2Li + CH4

But what about those other products, CH3SOLi, CH3SOCH2Li that were formed, any one have any information on the color of these compounds possibly to explain the red/black/brown plume rising from the cathode maybe the lithium reduced the DMSO to DMS? And how about methyl lithium, supposedly it is a somewhat common organic reagent and somewhat stable, how fast would anyone here guestimate the rxn between the methyl lithium and DMSO would be in terms of a rate?

Really, I must try this experiment again, it was very interesting to say the least. Numerous color changes, lithium metal, many lithium-organic compounds in solution. How about any other ideas as to the identity of the gas produced at my cathode? The information that I have on DMSO reacting in this manner with NaCl states that gas evolution should come from the anode, however logic would dictate that the lithium would be produced at the cathode and react with the DMSO there, why would it have to react at the anode, that part is a chemical reaction, not an electrochemical reaction.

The_Davster - 17-5-2004 at 19:13

I'm not really sure but...
When the Ni becomes Ni2+, the Ni2+ replaces Li+ as the strongest oxidizing agent so it will be preferentially plated onto the cathode before lithium metal. your black coating could just be a fine layer of nickel plating. Why did you choose a nickel anode and not graphite or another inert electrode? I am not sure what the gas formed was.
This may be too simplistic an explanation or not aplicable.

[Edited on 18-5-2004 by rogue chemist]

BromicAcid - 17-5-2004 at 19:21

I know I did get some lithium but yes, I did neglect that the nickel could just be re-plating on the cathode. I used nickel because I bought a 2 Kg roll of nickel wire awhile back and I made 100 .3m electrodes from it, so they are essentially stock piled. I will have to run this electrolysis with an inert electrode. Still though, the colors in the solution are perplexing, it turned almost black but a ml or two of water turned it just to a faint blue of nickel salts.

BromicAcid - 22-5-2004 at 17:22

Today was my day of electrolysis of LiCl in non-aqueous mediums.

In DMSO: Tried this again with a graphite anode to prevent it from reacting. It greatly slowed the reaction from what I was getting with the nickel anode, possibly the nickel cations were adding to the mobility of the electrons through the solution. But electrolysis did proceed, albeit slowly. Also there was no color change at the cathode as there was before although gas evolution was noted as before. After quite some time I removed the cathode and there was no noticeable deposit, it did bubble somewhat vigorously for a second when water was spritzed on it but whatever was there was present in sub-gram amounts.

In Acetone: The reaction was almost nonexistent as judged by the amount of bubbles produced. Though there was a steady stream, it was nothing considering I was throwing 12V 10A at it, solution finally obtained a very light haze to it but there was no cathode deposition. The electrodes were very nearly touching in solution.

In Acetonitrile: Solution was nearly nonconductive, worst conductivity of the lot, electrodes were a hairs width apart and a bubble would emerge every few seconds.

In Nitrobenzene: Second worst conductivity of the lot. Ran the reaction for a few minutes with almost no indication of reaction and my heart skipped a beat when the electrodes touched under the solution and it sparked. I knew dinitrotoluene can explode even though it is highly oxygen deficient so I had to worry a bit. No reaction at all in terms of a cathode deposit. (Also, I didn't know I could get a nitro headache just from the occasional waft of nitrobenzene vapors, well, live and learn)

In Methanol: This one was just for fun. The reaction was incredibly fast, the bubbles were coming up like tossing a piece of Mg into HCl. The solution took on a yellow color very fast and the solution clouded up. The solution was boiling and electrolysis was discontinued. A precipitate settled to the bottom.

Additionally not relating to this thread I tried NaBr in DMSO. The cathode bubbled but the anode turned orange/yellow and a solid started to continually flake off it. Overall DSMO actually gave the best results. And with the graphite anode the solution stayed clear although the cathode did take on a black color as before. Perhaps I could take what I have learned and try a mixed solvent?

[Edited on 5/23/2004 by BromicAcid]

Proteios - 1-6-2004 at 13:22

maybe THF is a good choice.....
literature drying of THF is over Na/K alloy....so its gotta be stable to the group 1 metals.

Dunno what conc. of Li salts you can get into THF... but I know for certain, lots of the Cs salts are really quite soluble in THF..... if you feel very brave.

BromicAcid - 1-6-2004 at 14:08

I've found references to 1 M LiCl solutions in THF so it is therefore somewhat soluble. If I had some THF I'd give this a shot.
Quote:
lots of the Cs salts are really quite soluble in THF..... if you feel very brave.

Nothing brave about it, it's just that cesium salts are usually quite expensive :(

Proteios - 1-6-2004 at 18:31

An interesting problem!
However I would still reckon that the cost of the Cs salt itself would be nominal compared with the cost of isolating the Cs. It would take a brave man to make more than 5g of Cs.... probably need to seal it in a ampoule...... vac line to get rid of the solvent... do the whole electrolysis under Ar or something to keep oxidation down..... tricky buisness!

Actually now that i come to think about it Cs melts well below the BP of THF..... just do the electrolysis in degased THF..... Ar atm. with the cathode over a test tube (at 40 C or something)... and with luck the molten Cs will pour off into the test tube..... simple eh?

Incidentally Ive been in chemistry a long time, and have never come across, or thought about isolation of group 1 metal by electrolysis of non-aq. solution... its a really neat idea :)

Marvin - 1-6-2004 at 21:20

A slightly more conventional idea for Cs might involve heating its chloride with calcium in a decent vacuum. Condense it directly in the ampule.

Proteios - 1-6-2004 at 22:20

Quote:
Originally posted by Marvin
A slightly more conventional idea for Cs might involve heating its chloride with calcium in a decent vacuum. Condense it directly in the ampule.


CsCl dont melt till 600 and Ca 800.... Cs boils 650... what kind of reactor do you know that holds a good vacuum at this sort of temperature??? Ca and CsCl woundt react at RT.... dunno about 600 C though.
In terms of conditions..... 40C, and a mild DC current would seem more accessible conditions that 0.5 thousand C... esp. when dealing with a chem. that is violently oxidised.

Marvin - 2-6-2004 at 23:21

I'm not convinced its boiling point has much relevence in a vacuum, but melt one of them and there will certainly be a reaction even if there isnt in the solid state.

Stainless steel for preference, quartz tube, but if I was doing it for small amounts Id probably suspend a little metal crucible in a flask and heat it electrically. Keeping the whole thing inside a bag of inert gas would be good idea, that way if the flask implodes there isnt a risk of explosion.

Reduction with calcium has a number of advantages, its quick, its pure and not least we know it works. RT organic solvent electrolysis would have some uses if the electrode current density can be made high enough to produce at a reasonable rate, but this assumes it works at all.

"0.5 thousand C"

Can you make that sound any more impressive? Gee, thats... thats... One and half thousand degrees Rankine!

It is violently oxidised, such as by oxygen dissolving in the solvent and the oxidised products forming at the other electrode... I cant help but wonder if there would be problems with something as simple as sodium or potassium being produced quantitivly.

BromicAcid - 25-10-2004 at 08:48

Trying lithium chloride in DMSO again under more controlled conditions.

An excess of LiCl was added to 25 ml of DMSO and placed in a test tube. .05 g of Na metal was added to try to ensure the solvent to be somewhat anhydrous, and although sodium reacts with DMSO on it's own, the reaction was very slow, leading me to believe water contamination was not extensive.

A rubber stopper was put into the top of the test tube and two small holes were made to allow for two nickel electrodes to enter the solution. Electrolysis was begun, 6V, 300 ma and has been going for 30 minutes as of now.

The cathode is covered with a black substance and bubbles continuously, as usual the anode is going into the solution and sinking straight to the bottom. There is a very sharp division in the color of the electrolyte, the top layer, about 3/4 of it, is dark brown now, and the bottom 1/4 is light blue with not a hint of brown, going to let this go another 8 hours or so and see what I end up with.

One of the products depositing or coloring the solution might be methyl lithium, anyone know a way I could test for this?

Edit #1: An hour has passed since this post. The solution no longer looks brown, it is now a very deep red through the top 3/4 of the test tube. The blue at the bottom has yet to mix. There is lots of solid dispersed throughout the mixture now, dark red flakes. I saw the top of the mixture and was ecstatic for a moment upon viewing the beautiful clear crystals that were appearing there, till I realized it was just my DMSO freezing. It was carefully heated as to not disturb the two layers, and now I leave it for another hour.

Edit #2: It's been going for over 2.5 hours so I went out to check on it. The red flakes had settled out somewhat to the bottom of the red layer and the blue layer remained separate. I decided that I should take some pictures, so I did. Then I decided that I wanted to stir it up, maybe the lithium percentage in the solution had dwindled and the exchange with the bottom solution was too low. So I took out the stopper... wait... tried to take out the stopper, the test tube broke when that happened. And guess what, I got a few ml's of that solution containing who knows what on my hand. DMSO solutions of lithium ions and more are not nice. Pure DMSO actually works considerably less effectively at transporting ions across the skin barrier, it works best in the 85 - 95% range when combined with water. So I dashed to my shed and rinsed with acetone, then water. I think I'm starting to get a headache. Nevertheless, I got a new test tube, retransferred the solution, now a homogenous color and consistency to a new test tube and recommenced electrolysis, I'm eager to see if it resettles. (Note, the electrodes once removed gave no indication of lithium, in my previous runs there was evidence of it, possibly high currents are necessary to deposit it faster then it reacts with its surroundings.)

Edit #3: A little over 3.5 hours have passed. The solution has somewhat resettled. There appears to be a difference in density of the solution, the solid has settled somewhere in the lower area of the test tube, but not at the bottom. There is no longer a distinction of colors evident, it's all red, but I can see into the solution now that the solid has settled. I can taste DMSO, but my headache went away.

Edit #4: And thus it continues. Everything settled out. There was a thick layer of whatever the reaction is making on right above some of the solid LiCl remaining in the test tube. The solution was dark red, but did not contain appreciable suspended material. It is still going. I shook the reaction mixture and now it looks like mud. But it's already starting to settle, I think the precipitate is aging nicely and settles easily as a side effect.

Edit #5: Total of 5 hours has passed. I removed the electrodes, no trace of lithium. Thinking that I may have somehow formed a lithium complex imbedded in a sulfur crown I added some of the red liquid in some benzene to see if any of the color would transfer over, no. Added some of the precipitate to water, the solution went clear but the precipitate made a suspension. The whole mixture heated up, not a lot, but it heated up somewhat. That's it, done with DMSO for today.

[Edited on 10/25/2004 by BromicAcid]

vulture - 5-11-2004 at 14:00

Lithium batteries use a mixture of ethylcarbonate and dimethylcarbonate as elektrolyte for the Li<sup>+</sup> ions...

Dimethylcarbonate isn't very expensive, I could only find diethylcarbonate at acros.com though...

unionised - 6-11-2004 at 14:10

I think DMSO is doomed.
http://www.casper.organ.su.se/sop/sop401.html

BromicAcid - 10-12-2005 at 09:59

Looking through a book yesterday titled "Industrial Electrochemistry" I found the lithium section to be fairly interesting and decided to reproduce it here:
Quote:
Lithium Electrowinning
Lithium is prepared by the electrolysis of fused lithium chloride in a lithium chloride - potassium chloride bath at 400 to 450C held in a cell designed somewhat like a Dow magnesium cell or the Downs cell for sodium production so that the intermixing of the lithium metal and the chloride gas is prevented (See Magnesium Electrowinning and Sodium, Electrolyte Production.) The LiCl-KCl mixture is approximately the eutectic mixture (about 45 per cent LiCl) whose melting point is 352C; the melting point of LiCl is 606C. Compared with the use of fused LiCl alone, this mixture improves optimal efficiency, decreases corrosion problems, minimizes deteriation of the graphite anodes, and permits continuous operation.

The raw material is lithium chloride of high purity, particularly with respect to water and sodium content, although water can be removed to a degree from the bath by pre-electrolysis at low amperage. Since lithium chloride is very hygroscopic, the handling of it to deter water pickup is a problem.

The physical properties of lithium and the LiCl-KCl eutectic mixture influence the cell design. Lithium melts at 179C and at 400C has a density of 0.49 g/cc, a viscosity of 0.402 centipoises, a vapor pressure much less then 1 mm Hg, and a surface tension of about 400 dynes/cm. The eutectic mixture has a density of 1.65 g/cc at 450C and a viscosity of 5 centipoises at 500C. Lithium chloride has a decomposition potential of 3.684 v at 450C calculated from thermodynamic data, and the formal electrode potential for Li<sup>+1</sup> in eutectic LiCl-KCl at 450C is -3.41 v measured against a Pt, Pt<sup>+2</sup> reference electrode. (See Fused Salt Electromotive Force Series.)

One type of cell used commercially is constructed of a covered steel pot suspended in a firebrick heating chamber, much like the magnesium cells. Gas or oil is used to heat the cell. Top entering graphite anodes dip into the fused salt bath, and the steel cathodes are so proportioned that the lithium rising from them to the surface of the bath is prevented from approaching the chlorine gas rising from the anode. Separate collecting means are used for withdraw of the lithium and the chlorine. The molten lithium is carefully protected from contact with air, and is withdrawn from a collecting vessel and cast into molds.

Another type of cell described recently<sup>1</sup> is designed like the Downs sodium cell. It is a covered, brick-lined cylindrical pot 26 in. in diameter and 30 in. deep with a single bottom entering anode 6 to 8 in. in diameter centered vertically in the pot. A steel cylindrical cathode 9 to 12 in. inside diameter and 8 to 12 in. high surrounds part of the anode, and between them is a cylindrical diagram of perforated 24-gague, 316 stainless steel sheet, which keeps the chlorine rising along the anode from mixing with the lithium rising along the inside of the cathode. A vertical hoodlike nickel chlorine collector is positioned over the top of the anode, and a steel collector placed over the cathode is used to hold and guide the molten lithium to a vertical takeoff line continuously into a stainless steel holding tank. Auxiliary electric heating elements in the bath maintain the temperature.

The lithium cells hold only a few hundred pounds of bath, and the production rate from cells using 900 to 1000 amperes is in the range of 8 to 10 lb of lithium per day per cell.

Some typical operating data for commercial cells are given in table 1.

The cell described in Ref. 1 operates at somewhat lower voltage, current density, current efficiency, and unit energy consumption, and its chemical efficiency is somewhat higher. While designed to operate at 1000 amperes, it can be operated up to 3500 amperes with no abnormal behavior.

Table 1. Lithium Cells-Operating Characteristics<sup>2</sup>
Current (amp) 850-900
Temperature
C 400-420
F 752-788
Voltage 8-9
Anodic c.d. (amp/sq. in.) 9.0
Cathodic c.d. (amp/sq. in.) 13.0
Current efficiency (%) 85-90
Unit energy (kwhr/lb) 18.2
Chemical consumption (LiCl/lb Li) 7.3
Chemical efficiency (%) 83.7
Cell capacity (lb) 220

Details about cell operation and about the physical properties and electrochemical behavior of lithium and its salts are presented in Refs. 1 and 2.

The separation of lithium isotopes 6 and 7 can be effected by the electrolysis in a mercury cathode cell and by electromigration techniques. Information about both methods is given in the article. Isotopes-Electrochemical Separation; also see Electromigration in Liquid Metals.

References

1. Motock, G.T., Electrochem. Tech., 1, 122-127 (1963)
2. Landolt, P.E., and Sittig, M., chapter on "Lithium" in "Rare Metals Handbook," C.A. Hampel, Editor, New York, Reinhold Publishing Corp., 1961.

Clifford A. Hampel
Makes designing and operating a cell to afford lithium metal from the chloride almost sound reasonable eh?

Fleaker - 16-12-2005 at 13:31

I have maybe 30 grams of lithium carbonate that I can dedicate to this reaction. I will use 300 mesh Li2CO3, 700 mesh Aluminum powder (in stoichiometric ratios) and what I deem to be enough magnesium oxide to moderate the reaction rate. Up until that point, I'm not too worried, but my problem is collection.

Since molten lithium is one of the most corrosive materials known, how should I contain the reaction? I was going to do it in a large evaporation dish in a sand bath with a watch glass covering it. I was planning on filling the evap dish with dry ice/MeOH so that the lithium vapor would deposit on the underside immediately (hopefully sparing the container). Eitherway, I'm worried about thermal shock. I hope the reaction is hot enough to vaporize the lithium metal (which would facilitate separation) but not too hot to crack the porcelain and the watch glass. I think I might use a taller reaction vessel or maybe use something with more thermal resistance than a flint watchglass. Any suggestions?

IrC - 16-12-2005 at 13:57

Correct me if I am wrong but lithium will burn in sand, by pulling the oxygen right out of the silicon dioxide just like magnesium does. I think you need an argon filled chamber. As far as I know burning lithium will even burn the oxygen out of glass. Fact is I don't even know how you would put lithium out, it will suck anything oxygen or nitrogen (which makes a really explosive nitride) right from wherever it can get it. I have two bottles each with 5 gm Li metal under oil I have never used as finding a safe way to do anything with it is hard. It makes me wonder why the chinese are so cavalier with all the toys on the market using big Li ion cells. I have a radio controlled helicopter which loves to crash and I was waiting for the day one of the cells starts burning. You should read the fire statistics in the U.S. for lithium batteries, mostly from improper charging using something like nicad chargers instead of the proper source. Come to think of it lithium is fun stuff after all! Think of the fireworks we can play with, of course blaming it all on a bad battery when the pyrotechnical police come looking for us.

neutrino - 16-12-2005 at 19:13

Liquid lithium is one of the strongest reducing agents known, if not the strongest. I doubt it could be obtained by a simple thermite reaction, although this one does involve distillation...

I doubt it will work, but it's worth a try.

Also, I think magnesium salts would just react with any lithium formed and liberate magnesium.

vulture - 17-12-2005 at 07:55

Well, lithium has the most negative reduction potential at STP, but in a thermite reaction there are lots of things that can shift the balance. The high stability of MgO and Al2O3 could shift the reaction, them being refractory oxides with high lattice energies.

Fleaker - 17-12-2005 at 09:21

I was going by what bromic posted:

"Reduction of LiOH or Li2CO3 or LiCl with magnesium as stated in Complete Treatise on Inorganic Chemistry is explosive but 40% magnesium oxide can be added to moderate the reaction. Information relating to chemical reduction by Mg or Al can be found if you see Warren, Chem. News, 1896, 74, 6, and U.S.P. 2028390. Lithium salts such as LiNO3, Li2CO3, and LiOH can be reduced with carbon or metal carbides or even calcium at high temperatures. Zirconium is an effective reducing agent for nearly any alkali metal that is combined with oxygen, it will reduce sulfates and phosphates in a self sustained reaction."

And to clarify, yes, I will be doing this under deoxidized argon but perhaps I will use alumina for the reaction vessel.

neutrino - 17-12-2005 at 10:28

Yes, you're right. I forgot that standard potentials are only valid at STP.

BromicAcid - 8-4-2006 at 18:42

Okay, going off what I posted earlier about lithium chloride electrolysis, 10 grams of lithium chloride and 11 grams of potassium chloride were placed into a steel crucible. The two components were heated with a propane torch and fairly rapidly the bottom of the mixture liquefied and within a few minutes it was entirely liquid. It was at this time that the crucible was connected to the power supply and made into the anode of the circuit and a nickel rod was made into the cathode.



So, immediately the nickel wire coated itself in the melt and refused to perform electrolysis considering it was much colder then the surroundings so I scraped it on the bottom of the crucible until it made a connection (evident by the amp meter shooting up past 15) and then raised it up slightly whereupon bubbling became very rapid (the usual spray of bubbles). Nothing much happened at first, likely water was being electrolyzed as is the case with most of these melts and it is also mentioned as a possibility in the outline of this technique mentioned earlier.

Finally the area surrounding the cathode quickly glowed red and the amps being consumed shot up past 15 and popped the fuse in the power supply. Success, lithium likely formed in the shallow space between the anodic crucible and the cathode right above it. After the circuit breaker kicked back in I tried again, just the slightest contact of the cathode with the surface of the melt instantly rose the amps consumed past 10 so the melt is highly conductive. As soon as the wire touched the surface a red glow would spread out and occasionally pop sending out glowing embers or fire would sputter up (see the glow in the picture above).

This was just a proof of concept after all. Although I did expect it to work. There is great promise in this technique in that temperature control is not as necessary as it is in electrolysis using the metal hydroxide and I've been working on the problem of separating the products.



That up above is my cell that I will be using soon. A simple U-tube with a stopper in the cathode compartment to prevent lithium from reacting with the air. And also a stopper in the anode department with a glass tube in it to lead away the chlorine produced into a suck back bottle and then into a base wash to decompose it. I used a similar cell for electrolysis of potassium hydroxide with good results. So hopefully this will work. The only problem being that the lithium formed will be inaccessible while the reaction is running so I can only run it till I get a small ingot (at which time the cell will likely draw considerably more current due to the lithium acting to expand the electrode area) then I will have to cool it down, take it apart, and take out the lithium.

On advantage we don't have with the sodium hydroxide cell is that glass will hold up to these temps (at least borosilicate) on disadvantage is that lithium will attack glass so that's again put out of the question. But I was wondering about high temperature silicones and such should I need a diaphragm if I change the construction. Nonetheless, just updating those interested on my progress in this area.

Marvin - 9-4-2006 at 15:53

Did you get any lithium formed that could be identified after the reaction or could it have been a lithium potassium alloy?

BromicAcid - 9-4-2006 at 18:10

I could have swore I read somewhere that lithium and potassium don't form an alloy akin to the alloy formed between sodium and potassium, but that could likely be a figment of my imagination. Anyway, I got no indication that it was lithium formed over an alloy or even over potassium. I got a red glowing spot that occasionally caught fire and skittered around but nothing confirmatory. The crucible as you see was deep and the chlorine was being generated all around it (though I think a lot of the chlorine formed just ate the crucible, there was smoke which could be FeCl<sub>3</sub>;). So there was no confirmatory aspect to it.

What might be useful would be a watercooled cathode. I think there is something of the like in use for calcium electrolysis where it is slowly pulled from the surface and as it is the calcium solidifies and you end up with a rod of calcium. I didn't really investigate the solid that was left after the melt cooled, it was very resistant to impact so I left its investigation for another day.

enhzflep - 9-4-2006 at 21:00

With research, photos and concise descriptions of your experiments you have many fans, BromicAcid. I for one always enjoy reading your posts, having become familiar with the quality of analysis presented.

Was just reading 'bout your dilema and i stumbled accross this
site:
http://www.njscuba.net/artifacts/matl_metallurgy.html

Anyway, it's been too long since i did chem (10yrs ago @ school) but since Li Na and K are all in the same period(?) (column), and are all metals with similar properties, i don't see why they couldn't form an alloy. Sure, maybe not one with definite Chem formula like with Na and K, but never the less, seing as Al and Au can be alloyed i see absolutely no reason for this not to be possible. They may just form what the above link calls a heterogeneous mixture of tiny crystals, as opposed to the true chemical compound that Na + K form. I suspect that all the mentions and uses of this alloy are due to its stronger bonding, and hence better integrity under high heat conditions - as found when using as a heat transfer medium. Hope this helps you that has helped so many.
cheers, enhzflep

S.C. Wack - 4-2-2008 at 03:02

A CELL FOR THE PREPARATION OF SMALL QUANTITIES OF ALKALI METALS
J. Chem. Ed. 31, 515 (1954)

http://www.box.net/shared/3c1ju8z6i9

S.C. Wack - 4-7-2009 at 11:57

Repost of the above by request.

http://ifile.it/skohwq0

Lithium/Al Alloy

WGTR - 30-10-2013 at 14:18

In the electrolysis of alkali metals, it seems that one thing that
makes isolation of the metals difficult is that the metal product
is a liquid in the molten salt bath and it floats, making
containment awkward and somewhat dangerous. I've
electrolyzed small mounts of lithium before in a LiNO3/KNO3
eutectic mix at about 150°C, allowing the lithium to remain
solid. This was still difficult, because the anode products acted
aggressively against graphite and stainless steel anodes.

In the electrolysis of hydroxides, a nickel anode can be used. In
a chloride/bromide melt, a graphite anode can be used. The
advantage of these types of melts is that the anodes don't
suffer significant deterioration in normal operation, and they
are fairly attainable.

Here is a phase diagram for Al-Li. Note that the temperature is
plotted in Kelvin:
Al-Li.jpg - 59kB
According to the diagram, aluminum melts close to 660°C, and
lithium melts close to 173°C. An alloy of the two, Li-80%/Al-
20% (atomic %) melts at about 490°C.

Below is a LiCl/KCl phase diagram plotted against degrees
Centigrade:
KCl-LiCl.jpg - 61kB
Between the range of 47%-77% mole % of LiCl, the salt
mixture remains molten below 490°C.

It seems conceivable that two anodes could be used: one
graphite, and the other aluminum. The anode current could be
split between the two of them, such that a solid alloy of 80%
lithium deposits at the cathode. If the cell was run at, say
450°C, then both the cathode and anodes would remain solid.
The LiCl concentration could start at 71%, and operate down
to 48% before extra salt would need to be added.

What could be done with an 80% alloy of lithium and
aluminum? It would be interesting to see how its reactivity
compares to that of pure lithium.

Anyway, here's a reference that details a process similar to
what I'm proposing. One big difference is that they deposited
lithium into an agitated molten aluminum cathode, and I'm
thinking of co-depositing the metals into a solid cathode:

Attachment: Lithium_Electrolysis_into_Molten_Aluminum.pdf (219kB)
This file has been downloaded 1041 times


Also, lithium alloy production by mixed salt electrolysis:

Attachment: 11031.pdf (1MB)
This file has been downloaded 1046 times


This reference:

Attachment: 81.pdf (286kB)
This file has been downloaded 1053 times

contains the following:
"Potassium chloride is the solvent and supporting electrolyte because it alone,
among the common alkali and alkaline-earth chlorides, has a decomposition
potential that is more extreme than that of lithium chloride. Put another way,
electrolysis of a melt comprising LiCl-NaCl will produce lithium metal containing a
substantial amount of sodium..."

So, electrolysis of a standard LiCl-KCl melt should not produce any potassium.

[Edited on 31-10-2013 by WGTR]

WGTR - 6-11-2013 at 15:06

Reading through http://www1.asminternational.org/asmenterprise/apd/help/Intr...
I realized that I probably misread the Al-Li phase diagram in my previous post.
If I'm not even more confused than I think, then it looks like a 70% Li alloy
remains solid up to 600K, a 60% alloy remains solid up to 800K, and a 50% alloy
up to 975K. At any of those temperatures, increasing the Li concentration causes
a molten phase to begin forming along with the solid phase.

Am I reading this correctly?

Motherload - 22-6-2014 at 11:56

I have been collecting Li foils from spent batteries. It isn't super pure but there still a fair amount in a spent battery.
How do I melt these foils down to get a lump ?
I can't seem to find much info on doing so.

elementcollector1 - 24-6-2014 at 19:40

I tried, it's not easy. Melting under oil at 200 C was insufficient.

PHILOU Zrealone - 26-6-2014 at 10:36

Could'nt LiOH be use straightforward? (just like NaOH or KOH)?
I'm the owner of two 50 kg drums of it from a big chemical warehouse sale... 50€/drum was fine for me ;) (yes 100€/100kg :cool:)

Just like the 1kg of AgCN for 1€, and the other chems I bought for a total of 2000€ (1€/kg or L) you don't get this often in one's chemist life.

[Edited on 26-6-2014 by PHILOU Zrealone]

WGTR - 26-6-2014 at 22:48

Here's my meager attempt at making lithium.

IMG_0116.jpg - 98kB

2.0g of Li2CO3 was ground together in a mortar with 4.3g of NH4NO3.


IMG_0096.jpg - 101kB

The resulting powder was heated gently in a test tube with a propane torch. Ammonia and carbon dioxide was driven off,
leaving molten lithium nitrate that gradually changed from dark brown to clear.

IMG_0097.jpg - 56kB

2.7g of KNO3 was added to the cooled down solid in the test tube, but the tube cracked upon reheating. For this
reason, the contents of the tube were moved to a small beaker, and reheated on a hot plate.

IMG_0102.jpg - 88kB

With the hotplate set at 300C, everything melted together as it was stirred with a stainless steel spatula.

IMG_0107.jpg - 98kB

For the anode, I choose platinum, because I can. Seriously, though, it was only $50, and it will last forever. The cathode
was just tin plated copper bus wire.

IMG_0108.jpg - 132kB

You can see the metal beginning to accumulate on the cathode wire, as well as the orange coloration from the NO2 gas.
The current was 300mA, and the voltage varied from 6-8 volts.
IMG_0110.jpg - 66kB

Here is a better picture, shown as more lithium has accumulated after about 30 minutes. It's dendritic in appearance, and
metallic looking. Keep in mind that we are using a KNO3/LiNO3 eutectic, that melts around 125C.
Lithium melts at 180C, so as long as we stay within that temperature window, the lithium remains solid in the melt. The
metal itself is protected by a thin layer of insoluble lithia, which is also a fast ion conductor for lithium ions.

IMG_0112.jpg - 418kB

Here's a short video for you that depicts the little explosions that would occur from time to time.

Attachment: burning_lithium.mp4 (1.8MB)
This file has been downloaded 981 times

Finally, here is another short clip. This one shows the reactivity of the metal with water. I noticed that it did not float, even in
spite of lithium's low density. I think this is because the metal deposit was not very dense, and was mixed with a considerable
amount of the much denser electrolyte.

Attachment: lithium_decomposition.mp4 (8.1MB)
This file has been downloaded 974 times

[Edited on 6-27-2014 by WGTR]

seilgu - 6-4-2021 at 18:38

Quote: Originally posted by WGTR  


For the anode, I choose platinum, because I can. Seriously, though, it was only $50, and it will last forever. The cathode
was just tin plated copper bus wire.



That is very misleading.

I think it destroyed my platinum wire, it seems to lost its shine after being used as electrode, even after cleaning with piranha solution and flame. Probably because lithium could form an alloy with the platinum, so it won't last forever. Lithium is known to be incompatible with platinum.

Also my quartz glassware was damaged by the burst of fire from the electrode, it formed a black spot and after cleaning I found that the surface of the quartz beaker had melted.

Nice experiment to destroy two expensive apparatus! I want my 20 bucks back!

[Edited on 7-4-2021 by seilgu]