Barium sulfate purification


Im purifying Barium Sulfate from Baryte rock.

Already have a procedure which I devised and am testing. (more later when all is done)

the question I have is:

"As barium sulfate is almost insoluble in water, digesting it with a concentrated NaOH solution (by digesting meaning: 1 hour, 70-80°C, 10M NaOH solution), the NaOH will not attack it"

Is this statement true?

The idea of this procedure is to remove SiO2 contamination from baryte, but leaving BaSO4 behind. I dont want to use HF.

or how much time/concentration is needed to make SiO2 soluble with NaOH.
(water glass projects use 4 to 8 grams of sodium hydroxide in 10 milliliters of water. i.e 10M - 20M; Nurdrage uses 80gr NaOH/100 ml - 20M - for 60gr SiO2)



[Edited on 1-7-2024 by RU_KLO]




Go SAFE, because stupidity and bad Luck exist.
View user's profile View All Posts By User
Sir_Gawain
Hazard to Others
***




Posts: 324
Registered: 12-10-2022
Location: Due South of Due West
Member Is Offline

Mood: Way less sad

[*] posted on 1-7-2024 at 16:56


One industrial method of obtaining barium compounds from baryte is heating with carbon to reduce the sulfate to sulfide, dissolving the sulfide in water, and precipitating barium carbonate or sulfate. The method you outlined should work, but will not provide as high purity. My best advice is to just try it.



“Alchemy is trying to turn things yellow; chemistry is trying to avoid things turning yellow.” -Tom deP.
View user's profile Visit user's homepage View All Posts By User
Precipitates
Hazard to Self
**




Posts: 70
Registered: 4-12-2023
Location: SE Asia
Member Is Offline

Mood: Acid hungry

[*] posted on 2-7-2024 at 05:27


Barium sulphate still has some solubility (2.4 mg/litre), and may react under such harsh conditions i.e. hot, very concentrated NaOH (which seems fair for dissolving silicon dioxide). But, if the loss in yield is small, it may be acceptable.

If the barium sulphate does react to a non-negligible extent, it may be worth just trying to dissolve all of it with the NaOH, and then adding hydrochloric acid to precipitate out the silica.

Then you can add NaOH to the barium chloride filtrate to recover barium hydroxide again. Depending on the visual purity you may want to perform a recrystallisation or two to remove iron (or/and alumina) impurities.

If you would then like barium sulphate, it can be obtained by reacting the hydroxide with calcium sulphate. Although barium hydroxide is a better starting point for barium compounds.

[Edited on 2-7-2024 by Precipitates]
View user's profile View All Posts By User
RU_KLO
Hazard to Others
***




Posts: 177
Registered: 12-10-2022
Location: Argentina
Member Is Offline


[*] posted on 2-7-2024 at 09:31


Quote: Originally posted by Precipitates  
Barium sulphate still has some solubility (2.4 mg/litre)....

If the barium sulphate does react to a non-negligible extent, it may be worth just trying to dissolve all of it with the NaOH, and then adding hydrochloric acid to precipitate out the silica.

Then you can add NaOH to the barium chloride filtrate to recover barium hydroxide again.
[Edited on 2-7-2024 by Precipitates]


It more difficult than this. You cannot go from BaSO4 to chloride directly.
(you need to convert it first to carbonate by refluxing long time, molar ratio 2:1 to 4.8:1 - Na2CO3:BaSO4 - depends on the source of information)

this is from our wiki:
The trick is that barium carbonate is even less soluble than barium sulfate, and sulfate can be converted to carbonate by lengthy boiling in a solution of sodium carbonate. This should be done under reflux, to prevent the solution in the pot from drying.

also BaSO4 solubility is 0.2448 mg/100 mL (20 °C) or 0.025 mg per liter...

the method for making/purifying BaSO4 soluble is in NaCl (840°C), up to 40% BaSO4 will dissolve in fused/molten NaCl.

Decant the impurities(in the molten NaCl) add Na2CO3 (4.8:1 ratio)
30 minutes and you have 95% convertion to BaCO3.

(the same procedure can be done with flourides (CaF2) to NaF/KF and gypsum to CaCO3 - but other alkaly earth halide should be used)

US2112903A
US2013401
Conversion of Barytes to Barium Carbonate
HAROLD SIMMONS BOOTH AND ELISHA FREDERICK POLLARD'
Western Reserve University, Cleveland 6, Ohio


[Edited on 2-7-2024 by RU_KLO]




Go SAFE, because stupidity and bad Luck exist.
View user's profile View All Posts By User
bnull
Hazard to Others
***




Posts: 300
Registered: 15-1-2024
Location: Between the Atlantic and the Pacific Ocean
Member Is Offline

Mood: Sleepy (again)

[*] posted on 2-7-2024 at 10:13


Quote: Originally posted by RU_KLO  
The idea of this procedure is to remove SiO2 contamination from baryte, but leaving BaSO4 behind.

Why not the other way around: dissolving BaSO4 and leaving silica as it is? A process is described in patent US1752244A, "Process for refining and purifying barium sulphate". I thought at first of EDTA or some other chelating agent but, inorganic salts being cheaper and easier to handle, the latter seem to be a better idea.

Attachment: US1752244.pdf (457kB)
This file has been downloaded 36 times




Quod scripsi, scripsi.

B. N. Ull

P.S.: Did you know that we have a Library?
View user's profile View All Posts By User
RU_KLO
Hazard to Others
***




Posts: 177
Registered: 12-10-2022
Location: Argentina
Member Is Offline


[*] posted on 2-7-2024 at 10:37


Quote: Originally posted by bnull  
Quote: Originally posted by RU_KLO  
The idea of this procedure is to remove SiO2 contamination from baryte, but leaving BaSO4 behind.

Why not the other way around: dissolving BaSO4 and leaving silica as it is? A process is described in patent


Just read it, it does not remove SiO2, it just make it easier to remove later "If silica or silicates are present in objection able amounts in the raw material, a mixture of sulphuric acid, with a small amount of hydrofluoric acid, serves to decompose and render soluble both the iron and the silica compounds.

Maybe I could add this procedure as starting procedure to make the baryte more "ready" to acid attack.




Go SAFE, because stupidity and bad Luck exist.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3631
Registered: 8-2-2015
Location: 3rd rock from the sun
Member Is Offline


[*] posted on 2-7-2024 at 11:20


'a small ammount of hydrofluoric acid' may passivate some contaminants making them difficult to remove later,
just guessing.




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
EF2000
Hazard to Others
***




Posts: 148
Registered: 10-5-2023
Location: The Steppes
Member Is Offline

Mood: Taste testing the Tonka fuel

[*] posted on 2-7-2024 at 12:06


If there are calcium compounds in baryte rock (and I guess there are), HF can turn them into CaF2, that is unfortunately insoluble and will be hard to remove. Same problem with strontium sulphate, celestine, that is often found with baryte.



Wroom wroom
"The practice of pouring yourself alcohol from a rocket fuel tank is to be strongly condemned encouraged"
-R-1 User's Guide
View user's profile View All Posts By User
bnull
Hazard to Others
***




Posts: 300
Registered: 15-1-2024
Location: Between the Atlantic and the Pacific Ocean
Member Is Offline

Mood: Sleepy (again)

[*] posted on 2-7-2024 at 13:45


Did you consult the references given in page 2 of the patent (see figure)? I can't give you any directions since the majority of the papers are in German, and my translations from it are sufferable at best. Perhaps you could adapt something from them.