[*] posted on 27-5-2017 at 23:37
cleaning vanadium


I have some nice vanadium crystals as part of my element collection. I did not take any particular care over their storage and now they have a green coating of ?oxides. What is likely to be the best way to clean them and get them back to their former glory ?. I will seal them under argon once clean.



If you're not part of the solution, you're part of the precipitate.
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6333
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 28-5-2017 at 00:29


I have never dealt with this particular problem -- My V sample is vacuum deposited crystals stored under argon.

Coincidentally, thiosoi2 (on yt) did a video this week on vanadium. He demonstrates cleaning crystals using nitric acid. Not sure of the concentration.
View user's profile View All Posts By User
nezza
Hazard to Others
***




Posts: 324
Registered: 17-4-2011
Location: UK
Member Is Offline

Mood: phosphorescent

[*] posted on 28-5-2017 at 01:20


Thanks for that. I'll give it a go with Nitric acid. I note in the video he says nitric acid will dissolve vanadium to give vanadyl chloride. I think he means aqua regia.



If you're not part of the solution, you're part of the precipitate.
View user's profile View All Posts By User
Neme
Hazard to Self
**




Posts: 86
Registered: 28-5-2016
Location: Czech republic
Member Is Offline

Mood: No Mood

[*] posted on 28-5-2017 at 04:47


In the comments he said that he used nitric acid and just did a mistake saying chloride.
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4618
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: PhD candidate!

[*] posted on 28-5-2017 at 05:58


Nitric acid does work very well for cleaning vanadium, as it does appear to be quite resistant to it. Even heating vanadium in nitric acid will only cause it to partially dissolve, to yield a faint blue solution, presumably vanadyl nitrate. However, I was successful simply using ascorbic acid to remove the oxide coating on the vanadium turnings that I have, with no noticeable damage to the metal at all.

On a related note, does anyone know why it is that vanadium metal is so hard to oxidize, while it is also hard to reduce solutions of it to the metal? Based on the behavior of its solutions I'd have expected the metal to have a reactivity similar to that of manganese.




Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
Texium
Administrator
Thread Moved
28-5-2017 at 05:58
violet sin
International Hazard
*****




Posts: 1482
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline

Mood: Good

[*] posted on 28-5-2017 at 18:11


The ascorbic acid worked great for me as well, shiny clean in no time, leaving a nice blue solution



View user's profile View All Posts By User
nezza
Hazard to Others
***




Posts: 324
Registered: 17-4-2011
Location: UK
Member Is Offline

Mood: phosphorescent

[*] posted on 29-5-2017 at 05:44


Thanks Guys. I liked the idea of using an organic acid as most are slight reducing agents and will not oxidise the Vanadium any further. Anyway I used Tartaric acid and these are the cleaned and washed crystals. I will now store them under Argon to keep them clean.

Vanadium.jpg - 298kB




If you're not part of the solution, you're part of the precipitate.