Lead refining failures


Hello everybody!

I tried recorvering some pure lead from range scrap in this video:

https://youtu.be/_KqRFpDpKoo

As you can see I might have messed up a little.

The question I wanted to ask if anybody has a good idea on how to extract the remaining 4kg of lead. I though of something like using Acetic acid to dissolve it and then get it back purified via elektrolysis. Does anybody have any better ideas?
My main worry with that is that the acetic acid when heated is going to dissolve copper and brass from the bullet shells too and ruin everything. You might be able to precipitate the copper out of solution using citric acid though.
View user's profile View All Posts By User
Chlorine
Hazard to Self
**




Posts: 56
Registered: 26-11-2016
Location: Maine, USA
Member Is Offline

Mood: Brominated

[*] posted on 26-11-2016 at 16:44


The easiest way to process the range scrap is via melting, most back yard foundaries will be able to melt lead, you just need to make sure you separated the rocks and the rounds. It wouldnt be practical to use any acids. I speak from experience when I say that melting works the best.
View user's profile View All Posts By User
NitratedKittens
Hazard to Others
***




Posts: 131
Registered: 13-4-2015
Location: In the basket with all the other kittens
Member Is Offline

Mood: Carbonated

[*] posted on 28-11-2016 at 03:30


But how will melting purify lead




Basket of kittens for you ........BOOM
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4673
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: Preparing to defend myself (academically)

[*] posted on 28-11-2016 at 08:09


Melting lead will purify it to an extent because the non metallic slag will float to the top where it is easily scraped off. It will not remove metallic impurities though. Most commercial lead is alloyed with antimony to harden it, and this will stay with the lead when melted. The only way to remove it as far as I know is by dissolving the lead in nitric acid. The antimony is oxidized and precipitates as antimony trioxide, which can be saved for other experiments.

Acetic acid alone will not dissolve lead. Peracetic acid will react vigorously with lead to give some lead acetate, but mainly it seems to yield an insoluble oxyacetate. Nitric acid is really the only surefire way of dissolving lead.




Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
Bert
Super Administrator
*********




Posts: 2821
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 28-11-2016 at 08:30


FYI- Melting and then FLUXING the lead to reduce the oxides will provide a bit better economy... Cover the surface of the melted lead with a good layer of sawdust, or some other carbonaceous material and stir with a wooden stick, perhaps even add a few chunks of beeswax or paraffin if particularly oxide contaminated. The ash and carbonized sawdust layer remaining floating on top will help keep the Lead/Lead alloy somewhat protected from O2 and provide some protection from re-oxidizing while you work with it.

Molten Lead is best poured from the BOTTOM of a smelter or ladle, with such a protective layer floating on top- Tools like these are nice.

Rowell Ladle:

(Edit)
Watched your video. Safety comments left on video... You were damned lucky not to be hurt badly, be more thoughtful and prepare better next time.

[Edited on 28-11-2016 by Bert]

31sJQvn2UJL.jpg - 14kB




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 28-11-2016 at 11:11


What a superbly simple idea !

Gotta make me one of those ladles.

A bit of annealed copper pipe should do for the spout.




View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 28-11-2016 at 11:41


LOL.

I just watched the video too. Dangerous, but entertaining.

Nice to see you guys learning (albeit slowly !) and enjoying lead casting.

Some PPE would have saved your Eyes if those lead-bombs had exploded at a slightly different angle.

Heating the mould is obviously a good plan, as you discovered.

Scraping the dross (s**t) off the top of the melt with a spoon is a good way to remove a lot of impurities.

Putting a steel lid on top of the crucible stops bits of wood and charcoal getting from the fire.

Finally, round pancakes are hard to get back into the crucible, so get some sand and make rod or bar shaped lead ingots instead. Even small 'muffin tin' shapes fit easier, and they are not so heavy.

Please DO NOT try melting aluminium, brass, copper or steel before you get used to how molten lead works, or before you buy some protective clothing !

(some of those mistakes Could have ended up with someone Very badly hurt if it was Al. Certainly someone permanently damaged if it was Cu or Fe)




View user's profile View All Posts By User
Bert
Super Administrator
*********




Posts: 2821
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 28-11-2016 at 18:08


Angle iron makes a nice ingot mould, the ingots stack and interlock very nicely- See the pictures attached. Remember, if you weld end plates onto angle iron like this, do it at a slight angle (to provide what foundry workers call "draft"), easing removal of the solidified ingot-


ingot-molds.jpg - 47kB

lead-3.jpg - 138kB




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
RogueRose
International Hazard
*****




Posts: 1597
Registered: 16-6-2014
Member Is Offline


[*] posted on 29-11-2016 at 01:37


As Aga said, stay away from Al, brass and copper until you get more experience. You might be able to handle zinc as it acts a lot like lead in how it melts.

A tip for melting lead (or any metal) is to put a lid on the crucible (tin can) to both block ash from falling in and it helps keep heat in unless it is in an enclosed furnace surrounded/covered by flame.

If using a tin can it is best to take some pliers and pinch/crimp the little lip around the top (where the lid is attached) to make the pour much smoother (doesn't get caught on the lip).

It is also better (IMO) to add the lead in stages like cover the bottom by 1/2 inch, melt, add about 1 cup of metal (like a measuring cup - 8 oz), repeat. The molten lead will rise above melting point and quickly transfer the heat to the new lead. The thorough contact speeds the melting even faster than adding it all at once. It doesn't hurt to preheat the lead pieces in a pan (maybe as the lid to the melt pot) so it needs less heat to melt.

A good way to pour if you have no containers is to find flat, smooth concrete. sweep or vacuum the surface for best results. Pour a small sample to see if it flows (if surface isn't flat it can run faster than water). You can pour long strips or little "dolips". It is best to have the metal as close to melting point and not 100's of degrees over if pouring on concrete. A steel soup ladle works well for this.

I have taken hot zinc and poured it into a 5 gal bucket of ice water. the pour is a slow, thin stream and it makes some really interesting shapes. Pouring too fast makes the pieces stick together but slower pouring gives pieces ~1-4g in size each. I think lead will act similarly to this and I am curious if water temps will change the shape of the resulting metal. DO NOT EVER DUMP LOTS OF HOT METAL AT ONCE into water or ice it can explode or cause flash steam burns. Pouring on fluffy snow would be interesting as well.


If you decide to work with brass, I would recommend A LOT of research prior as I found it much more difficult than any of the other metals mentioned and have not yet successfully melted any. Zinc evaporates before copper melts so the Zn/Cu mixture of brass can lead to zinc boiling away and out of the brass.
View user's profile View All Posts By User
RogueRose
International Hazard
*****




Posts: 1597
Registered: 16-6-2014
Member Is Offline


[*] posted on 29-11-2016 at 02:17


Quote: Originally posted by Bert  
Angle iron makes a nice ingot mould, the ingots stack and interlock very nicely- See the pictures attached. Remember, if you weld end plates onto angle iron like this, do it at a slight angle (to provide what foundry workers call "draft"), easing removal of the solidified ingot-




Is that all lead? May we ask where you find sources for it? (PM me if you don't want to make it public).

I'd like to see a thread on refining battery plates from lead-acid batteries. Between the Lead sulfate and lead dioxide, it gets pretty tough but I'm really interested in the procedure with proper equipment like kiln, furnace or forge and possibly carbon as a reducing agent or acids for dissolving.
View user's profile View All Posts By User
Bert
Super Administrator
*********




Posts: 2821
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 29-11-2016 at 04:39


That is not my personal stash of Lead- I have only got about 400 lb. or so on hand, plus perhaps another 100 of various type metal alloys and about 20 of Tin.

Where to find Lead? Tire shops. Scrap yards. Dead people whos survivors had no interest in bullet casting. Construction workers remodeling clinics with shielded Xray rooms (that one was HUGE). Craig's List. Word of mouth. Scrounging in dumpsters.:P




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
ElchScience
Harmless
*




Posts: 17
Registered: 14-8-2016
Member Is Offline

Mood: No Mood

[*] posted on 29-11-2016 at 07:44


Wow crazy amount of Feedback thank you guys so much for all this! :-)

About the safety concerns: Yes we are aware that we didn't do all of this as safe as we could have done it. Next time we will make sure to not let any of these kind of failures happen. As for more safety equipment we are going to try to use a little more next time. You can't see it in the video but we did put on safety googles so worst case would have been a scar in the face. I am glad you guys are worried about our health and we will try out best. It is also in our best interest to not get hurt.

As far as crucible equipment and that kind of stuff goes: We didn't have any proper cast iron pots back then that we could use but now we do, so in the future this shouldn't be a big deal. We also don't have proper welding equiptment so we can't make our own molds, but the idea with the angle iron sounds really smart. Maybe a friend can help me with that. Thanks for the idea and all of the tips Bert!

I am not really convinced that the combination of molten metal and water is all to dangerous if the metal can't trap any of the water like in the mold. The leidenfrost effect should help out with that a lot. I am not saying that you don't have to be careful though. Always have a lot more water then molten metal and always be careful with anything you do!

Thank you Rogue Rose, aga and zts16 for all your tips!

Now back to my actual Problem of recovering the remaining 4kg or 9lbs of lead that are still in the scrap. They are very difficult remove by melting it again. That is why I thought of using acid.
zts16 and Chlorine are you sure that it is not possible to dissolve the lead in acetic acid? I have read on a german website that you can do it with a boiling solution of acetic acid. It could even be only 5% concentration. It apparently doesn't even require H2O2. Has anyone ever tried this? If not I will give it a shot.

Or is there a better way to get the lead that is stuck to the other gunk?

Thanks again everybody for all the amazing feedback! I am learning a lot here!

[Edited on 29-11-2016 by ElchScience]
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4673
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: Preparing to defend myself (academically)

[*] posted on 29-11-2016 at 08:30


Quote: Originally posted by ElchScience  
zts16 and Chlorine are you sure that it is not possible to dissolve the lead in acetic acid? I have read on a german website that you can do it with a boiling solution of acetic acid. It could even be only 5% concentration. It apparently doesn't even require H2O2. Has anyone ever tried this? If not I will give it a shot.
I haven't tried it, but I would expect it to be quite a slow process.



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 29-11-2016 at 08:39


Re-melt the lead and scrape off all the junk that floats.

This will remove the bulk impurites.

Cast the cleaner lead into beautiful Bert-style ingots ;)

If you have no mould, just use a bucket of slightly damp sand and press a shape into it with a stick.

The sand should be just damp enough so that it will hold a shape, but certainly not wet enough to stick to your hands.

Here's some Aluminium i did exactly that way (the sand-mould is something i just did to show you what i mean).

Al.JPG - 74kB

[Edited on 29-11-2016 by aga]




View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 29-11-2016 at 08:47


ANGLE IRON ! Of course !

Bert just gave me a great idea for another type of mould.

Cheers !




View user's profile View All Posts By User
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 30-11-2016 at 04:16


One can dissolve Pb (or even Ag), per my reported experience on SM, in dilute acetic acid/H2O2 (or use an air pump, in place of replenishing the H2O2, likely works also, but perform outdoors as Pb salt fumes should be avoided) plus an appropriate small amount of an electrolyte, after briefly jump starting the electrochemical reaction in a microwave, fairly rapidly. One can effectively use critic acid to form citrates as well.

Generally, for the electrolyte, I would recommend NaCl or sea salt, except in cases where the associated metal chloride (like for silver and lead) are insoluble, where I recommend KNO3 in place of NaCl.

Those in disbelief can forget the electrolyte and the microwave jump start and wait a week or more as I once did.

[Edit] I recall a reported instant of Lead induced brain fog suffered by a son helping his father who was breaking down Lead batteries, likely absent appropriate safety equipment. I personally have decided to avoid experimenting with Pb salts (more of an issue of potential toxic exposure to others and the environment).

[Edited on 30-11-2016 by AJKOER]
View user's profile View All Posts By User
Liamatpm
Harmless
*




Posts: 48
Registered: 7-12-2016
Location: Maine
Member Is Offline

Mood: Using the process of cellular respiration to stay (barely) alive

[*] posted on 9-12-2016 at 09:37


I would recommend watch some Cody's Lab stuff on YouTube. He has videos on refining of metals.
View user's profile View All Posts By User
Bert
Super Administrator
*********




Posts: 2821
Registered: 12-3-2004
Member Is Offline

Mood: " I think we are all going to die. I think that love is an illusion. We are flawed, my darling".

[*] posted on 10-12-2016 at 07:24


Might I suggest something a bit older school, and less materials required if these guys want to do many kilos of scrap bullet metals containing Tin, Antimony, Copper???

Liquation:

https://en.m.wikipedia.org/wiki/Liquation#/search




Rapopart’s Rules for critical commentary:

1. Attempt to re-express your target’s position so clearly, vividly and fairly that your target says: “Thanks, I wish I’d thought of putting it that way.”
2. List any points of agreement (especially if they are not matters of general or widespread agreement).
3. Mention anything you have learned from your target.
4. Only then are you permitted to say so much as a word of rebuttal or criticism.

Anatol Rapoport was a Russian-born American mathematical psychologist (1911-2007).

View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 10-12-2016 at 08:32


I got ripped off with some lead i bought a while ago, which turned out to contain 4 sacrificial anodes for boats.

'Liquiation' looks like it might work for splitting out the component metals, one of which is a bar of steel ...

Thanks for the link Bert !

SM is priceless for Gems of knowledge like these.




View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 11-12-2016 at 09:34


Turned out that the sacrificial anodes were just Zinc with a steel bar thru the middle so it can be bolted onto a ship's hull.

Never cast Zinc before. An amazing shiny finish without any effort at all !




View user's profile View All Posts By User
awlb2
Harmless
*




Posts: 27
Registered: 21-11-2016
Member Is Offline

Mood: No Mood

[*] posted on 12-12-2016 at 10:46


Digging gloveless hand around in sack of lead scrap and inhaling your lead 'incense' is insane. :o

World Health Organization: 'At high levels of exposure, lead attacks the brain and central nervous system to cause coma, convulsions and even death'



[Edited on 12-12-2016 by awlb2]
View user's profile View All Posts By User