[*] posted on 26-8-2015 at 08:36
anyway to recover and purify the zinc from old batteries?


Hi,
I was wondering (seeing as I have a huge amount) if there was any way to recover the zinc from old batteries like AA batteries and such? They are a wide mix of batteries including alkali and many other kinds. I looked at the Nurd Rage video on recovering MNO from old batteries but he mentioned that process couldnt be used on alkali batteries.
Alot of the batteries are corroded so I was thinking maybe some kind of electrolysis method? I wouldnt normally bother but the school collected huge numbers in a recycle bin but the company that supplied it didnt show up again! Sooo I scrounged them :D, probably not worth the effort but has to be over 1000 batteries I am sorting through to see if there is any lithium ones

LG




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 26-8-2015 at 14:04


Probably not worth the effort, unless you discover a quick and automated way to recover the components.

1000 is a lot of batteries, but if you work out the Time taken to process them, the results are simply not worth it.

Finding the Li ones would be most fun.




View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6372
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 26-8-2015 at 14:30


Electrowinning might be your best bet.
Melt your contaminated Zn into a crude ingot. Immerse as an anode into a Zn solution. Run a current and collect purified zinc at the cathode, catching impurities in your electrolyte.
Repeat as needed.
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 26-8-2015 at 14:46


Quote: Originally posted by j_sum1  
Electrowinning might be your best bet.
Melt your contaminated Zn into a crude ingot. Immerse as an anode into a Zn solution. Run a current and collect purified zinc at the cathode, catching impurities in your electrolyte.
Repeat as needed.


Thanks for that, I got a cheap graphite crucible that should do the job!

I have found loads of lithium batteries in the box, I am guessing I could build a box with gloves attached fill with N and take the lithium out if its in any fit state.
I want to clean the MNO as I am wanting to make a large home made battery with potassium hydroxide as electrolyte, no reason for it just kinda interested. MNO seems expensive at the mo




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 26-8-2015 at 15:34


Quote: Originally posted by Little_Ghost_again  

I have found loads of lithium batteries in the box, I am guessing I could build a box with gloves attached fill with N and take the lithium out if its in any fit state.


Spent Li batteries don't contain any Li metal anymore: it's all been oxidised, remember? It's what batteries do! ;)




View user's profile View All Posts By User
diddi
National Hazard
****




Posts: 723
Registered: 23-9-2014
Location: Victoria, Australia
Member Is Offline

Mood: Fluorescent

[*] posted on 26-8-2015 at 15:44


if it is an academic exercise then go ahead, but to be honest, you can buy 999 bullion of Zn for a few $ a pound, so why bother?



Beginning construction of periodic table display
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 26-8-2015 at 16:12


Quote: Originally posted by blogfast25  
Quote: Originally posted by Little_Ghost_again  

I have found loads of lithium batteries in the box, I am guessing I could build a box with gloves attached fill with N and take the lithium out if its in any fit state.


Spent Li batteries don't contain any Li metal anymore: it's all been oxidised, remember? It's what batteries do! ;)


Not all are spent, a fair few are showing above 1V.

Its a bit of everything exercise really.




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
Justin Blaise
Hazard to Self
**




Posts: 82
Registered: 5-10-2011
Location: Parts Unknown
Member Is Offline

Mood: No Mood

[*] posted on 26-8-2015 at 20:45


Quote: Originally posted by Little_Ghost_again  


I have found loads of lithium batteries in the box, I am guessing I could build a box with gloves attached fill with N and take the lithium out if its in any fit state.


Another problem is that Li reacts with N2 at room temperature. You'd need Ar ($$) for that job.

Edit: Glove bags aren't so expensive, though.

http://www.sigmaaldrich.com/labware/labware-products.html?Ta...

Alternatively, you could make one as per the attachment.



[Edited on 27-8-2015 by Justin Blaise]

Attachment: ed072p96.pdf (944kB)
This file has been downloaded 467 times

[Edited on 27-8-2015 by Justin Blaise]
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 26-8-2015 at 23:39


Quote: Originally posted by Justin Blaise  
Quote: Originally posted by Little_Ghost_again  


I have found loads of lithium batteries in the box, I am guessing I could build a box with gloves attached fill with N and take the lithium out if its in any fit state.


Another problem is that Li reacts with N2 at room temperature. You'd need Ar ($$) for that job.

Edit: Glove bags aren't so expensive, though.

http://www.sigmaaldrich.com/labware/labware-products.html?Ta...

Alternatively, you could make one as per the attachment.



[Edited on 27-8-2015 by Justin Blaise]



[Edited on 27-8-2015 by Justin Blaise]


We have a MIG welder and I think thats got Argon :D, I will check later




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
Keith Fletcher
Harmless
*




Posts: 29
Registered: 3-10-2014
Location: Eastern US
Member Is Offline

Mood: Brittle

[*] posted on 27-8-2015 at 07:53
Recovering Zinc from Zinc Carbon Batteries


Disassemble the battery remove the carbon electrode and then dissolve the zinc in Nitric acid or some other Mineral acid to make zinc nitrate. Then decompose the zinc nitrate to get pure zinc metal.

Zincbattery_(1).png - 92kB




My rule of life prescribed as an absolutely sacred rite smoking cigars and also the drinking of alcohol before, after and if need be during all meals and in the intervals between them.

- Winston Churchill
View user's profile Visit user's homepage View All Posts By User
gdflp
Super Moderator
*******




Posts: 1320
Registered: 14-2-2014
Location: NY, USA
Member Is Offline

Mood: Staring at code

[*] posted on 27-8-2015 at 10:47


Quote: Originally posted by Keith Fletcher  
Disassemble the battery remove the carbon electrode and then dissolve the zinc in Nitric acid or some other Mineral acid to make zinc nitrate. Then decompose the zinc nitrate to get pure zinc metal.

That's nowhere close to as simple as you make it seem. Zinc nitrate will decompose to zinc oxide and nitrogen oxides at moderate temperatures, but reclaiming the zinc from the oxide the way you propose would be quite difficult. Zinc oxide decomposes at nearly 2000°C, at which point the zinc would be gaseous. Condensing this without reoxidation would be nearly impossible on an amateur scale, and most certainly not worth the effort for relatively small amounts of zinc. Substituting the direct decomposition of zinc oxide with a carbothermal reduction would lower the necessary temperature to around 1000°C, but you still have the issue of condensing the zinc under an inert atmosphere to prevent reoxidation. Electrolysis of zinc sulfate may be plausible, and would certainly be easier than a high temperature reduction, see older relevant threads on SciMad.




View user's profile View All Posts By User
Keith Fletcher
Harmless
*




Posts: 29
Registered: 3-10-2014
Location: Eastern US
Member Is Offline

Mood: Brittle

[*] posted on 27-8-2015 at 14:07


2 ZnO + C --> Zn + CO2

https://books.google.com/books?id=tR9DAAAAIAAJ&lpg=PA38&...




My rule of life prescribed as an absolutely sacred rite smoking cigars and also the drinking of alcohol before, after and if need be during all meals and in the intervals between them.

- Winston Churchill
View user's profile Visit user's homepage View All Posts By User
diddi
National Hazard
****




Posts: 723
Registered: 23-9-2014
Location: Victoria, Australia
Member Is Offline

Mood: Fluorescent

[*] posted on 27-8-2015 at 14:17


re MIG gas: it often contains CO2. there is a pure Ar gas which is used for TIG welding, but you can use pure Ar in MIG, but it is dearer, so make sure you check carefully on the label.



Beginning construction of periodic table display
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 27-8-2015 at 14:29


Quote: Originally posted by diddi  
re MIG gas: it often contains CO2. there is a pure Ar gas which is used for TIG welding, but you can use pure Ar in MIG, but it is dearer, so make sure you check carefully on the label.


its my dads welder so I wont need to check, my dad being my dad is gonna go cheap, so I am betting its not pure :D....................


ran outside to check, just in case I was wrong about my dad being a tight arse.

Nope I was correct, it is not pure




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2171
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 27-8-2015 at 17:45


Lithium batteries are generally disassembled under
oil to recover the lithium. Where Little Ghost lives
it is probably legal. However in the 'Land of the Free',
it is illegal in some places.

As for the recovery of zinc from the oxide, this is
one of the earliest ore recoveries. The carbothermic
reaction occurs at modest temperatures but vaporized
zinc is a hazard although usually not fatal.
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 27-8-2015 at 18:22


Quote: Originally posted by macckone  
Lithium batteries are generally disassembled under
oil to recover the lithium. Where Little Ghost lives
it is probably legal. However in the 'Land of the Free',
it is illegal in some places.

As for the recovery of zinc from the oxide, this is
one of the earliest ore recoveries. The carbothermic
reaction occurs at modest temperatures but vaporized
zinc is a hazard although usually not fatal.


Thanks.
Any yep where I live most things are legal due to the seclusion :P.
In the uk you allowed to do most things except make ethanol (tax issue). Nitric acid (in case you hurt yourself). Hydrogen peroxide over 12% (in case you over bleach your hair).
Oh and breathing is to be heavily taxed. But no where can I find anything that says I cant take the lithium out of a battery, I cant go on a plane with a lithium battery but I am allowed to take it apart!
I cant buy Ammonium Nitrate in small quantity because of possible bomb making, but I am allowed to buy it by the ton for spreading on the fields here!

Mad times in Europe and UK


LG




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
Fluorite
Hazard to Others
***




Posts: 139
Registered: 26-12-2018
Location: United Arab Emirates
Member Is Offline


[*] posted on 26-1-2021 at 12:33


Sorry for being stupid but. Can I use battery zinc to make dimethyl zinc? If it claims 0% cadmium & mercury is it safe?
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5135
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 26-1-2021 at 13:13


"Can I use battery zinc to make dimethyl zinc?"
Yes

"is it safe?"
Not really. It catches fire on exposure to air.
View user's profile View All Posts By User
zed
International Hazard
*****




Posts: 2285
Registered: 6-9-2008
Location: Great State of Jefferson, City of Portland
Member Is Offline

Mood: Semi-repentant Sith Lord

[*] posted on 12-2-2021 at 07:37


Though on your Lithium Battery question, refer to NurdRage's Sodium preparations on Youtube.

A little salvaged Lithium is very useful for priming his Sodium producing procedure.

There are also Youtube videos on recovering Zinc from batteries.

Though there are other things in common batteries, that the guys find much more useful. Like Manganese Dioxide, and Carbon Electrodes. Are you OK with spoken English?

https://www.youtube.com/watch?v=knc1lSupAwQ

https://www.youtube.com/watch?v=XC5q9mDKUCo

Also, here in the U.S., our pennies are mostly made of Copper plated Zinc, so we don't really have a shortage.

It might be possible to generate Lithium via a Magnesium Thermite reaction. Seems to work for Sodium and Potassium.

As for Dimethyl Zinc, besides being highly flammable, I'm sure it is plenty poisonous. Kind of archaic really. Maybe used in Ketone synthesis, a hundred years ago? I used to read about such things, in ancient volumes of the Journal of the American Chemical Society. That, was back when I was a young Neanderthal, and we rode around on Mastodons. There are better ways of doing things now.

Though on inspecting Wiki, I find that Organo-Zinc compounds are used in plenty of applications, that most of us here don't usually think about.

Also of note: When I was a boy, we used to re-charge ordinary "Carbon" batteries. They lose their re-chargability after several cycles, but they were re-chargable.

At present, there is a device, that is purported to safely recharge alkaline batteries. I don't know what resources are like in Tunesia, but much of the world is currently feeling. "The Pinch".

I find this crusty old "Brit" entertaining. With his hand cranked, home-made Cell Phone re-charger.

https://www.youtube.com/watch?v=rozz-wbHfYM

About minute 18 or 19.

[Edited on 13-2-2021 by zed]

[Edited on 13-2-2021 by zed]
View user's profile View All Posts By User
DraconicAcid
International Hazard
*****




Posts: 4412
Registered: 1-2-2013
Location: The tiniest college campus ever....
Member Is Offline

Mood: Semi-victorious.

[*] posted on 12-2-2021 at 16:50


Quote: Originally posted by Fluorite  
Sorry for being stupid but. Can I use battery zinc to make dimethyl zinc? If it claims 0% cadmium & mercury is it safe?


All organometallic compounds are toxic (with the sole exception of one of the B vitamins). You do not want to mess around with the vast majority of them.




Please remember: "Filtrate" is not a verb.
Write up your lab reports the way your instructor wants them, not the way your ex-instructor wants them.