Titanium Dioxide Solution
Hey,
So, some time ago I saw two 1L bottles being sold for 30 cents marketed as a 4% Solution of Titanium Dioxide. They were plastic bottles and seemed
quite old and dusty. Inside there's a yellow liquid and a lot of white precipitate (TiO2 I guess). Anyway, for their price I just bought them.
Today I decided to open one and see what the liquid was and if the precipitate was indeed Titanium Dioxide.
Some propreties of the liquid:
-->The liquid is yellow (photo below) and has a faint smell of paint (organic solvent maybe?);
-->It is more viscous than water.;
-->It won't burn (not even with a blow torch);
-->I measured a density of about 0,996 g/cm3 give it or take it a few miligrams;
--> It's alkaline (turned litmus paper green);
-->I pippeted some of it into a watch glass and evaporated the liquid. What remained was some black stuff, carbon like (photo below);
I'm puzzled towards the identity of the liquid. Any thouhts? Has anyone ever come across such Titanium Dioxide solutions? Tomorrow I'll try to
identify the white precipitate (Titanium Dioxide I hope).
--------------------------------------------
Picture of the liquid:
https://www.dropbox.com/sc/ndp6wzcjxj1y0pu/AACZqV_DPs2UZ5JSD...
Pictures of the black stuff:
https://www.dropbox.com/sc/axeem1ascb5h8rt/AAAQg7ZxAYFVMign1...
https://www.dropbox.com/sc/phqm5tmqpg519fr/AAAAjLmX4Ybfd0V-_...
|
|
DrMario
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 332
Registered: 22-9-2014
Member Is Offline
Mood: Underpaid.
|
|
TiO2 is completely insoluble in water. It is also one of the least reactive chemicals in nature... and in the lab.
What you might have is some kind of suspension in water, using a surfactant (which would explain why it's a bit more viscous than water). It's also
possible that you bought a bottle of what is technically called "snake oil".
Could you snap a picture of the bottle/label on the bottle? That could prove very enlightening.
|
|
HgDinis25
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 439
Registered: 14-3-2014
Location: Portugal
Member Is Offline
Mood: Who drank my mercury?
|
|
The label is in portuguese so it be useless to you, I think. It simply says Titanium Dioxide in big letters and in smaller ones 4% solution. But yes
it seems to be a suspension of it. The surfactant idea seems plausible, might also explain the black residue left from boiling it (most of it boiled
away).
What compound might it be anyway? I'll check for miscibility with water tomorrow.
|
|
DrMario
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 332
Registered: 22-9-2014
Member Is Offline
Mood: Underpaid.
|
|
Quote: Originally posted by HgDinis25 ![](images/xpblue/lastpost.gif) | The label is in portuguese so it be useless to you, I think. It simply says Titanium Dioxide in big letters and in smaller ones 4% solution. But yes
it seems to be a suspension of it. The surfactant idea seems plausible, might also explain the black residue left from boiling it (most of it boiled
away).
What compound might it be anyway? I'll check for miscibility with water tomorrow. |
I do speak 6 languages, actually, and Portuguese is in the family of languages that I at least understand rather well.
What could the surfactant be? Polysorbate 20, sodium stearate, PEG 2000... something cheap, in any case, considering you paid 30 cents for one liter
of the goop.
|
|
HgDinis25
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 439
Registered: 14-3-2014
Location: Portugal
Member Is Offline
Mood: Who drank my mercury?
|
|
My strange liquid doesn't form a layer when mixed with water.
Does anyone know tests for specific sufactants?
PEG200 is probably out because my liquid doesn't seem to have a flash point. Sodium Stearate would need a solvent that would make a layer with water
(I think). Any thoughts?
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
You'll probably have to fuse (dry it thoroughly first) it with sodium bisulphate, that's how insoluble and inert it is. It's reactivity does depend on
grade to grade.
My food grade Anatase TiO<sub>2</sub> doesn't even respond slightly to 200 C 98 % H2SO4.
Once dissolved (if you manage it), dilute the solution and add aluminium foil or zinc (in a test tube!). That causes any TiO<sup>2+</sup>
(titanyl cations, Ti(IV)) to be reduced to purple/deep blue Ti<sup>3+</sup>.
Adding hydrogen peroxide then causes a deep red peroxo titanium (IV) complex to form.
[Edited on 23-10-2014 by blogfast25]
|
|
HgDinis25
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 439
Registered: 14-3-2014
Location: Portugal
Member Is Offline
Mood: Who drank my mercury?
|
|
Quote: Originally posted by blogfast25 ![](images/xpblue/lastpost.gif) |
You'll probably have to fuse (dry it thoroughly first) it with sodium bisulphate, that's how insoluble and inert it is. It's reactivity does depend on
grade to grade.
My food grade Anatase TiO<sub>2</sub> doesn't even respond slightly to 200 C 98 % H2SO4.
Once dissolved (if you manage it), dilute the solution and add aluminium foil or zinc (in a test tube!). That causes any TiO<sup>2+</sup>
(titanyl cations, Ti(IV)) to be reduced to purple/deep blue Ti<sup>3+</sup>.
Adding hydrogen peroxide then causes a deep red peroxo titanium (IV) complex to form.
[Edited on 23-10-2014 by blogfast25] |
Last time I worked with TiO2, pigment grade (is that even IUPAC aproved?), it dissolved in 300ºC Sulfuric Acid (near the decomp. temp.). Adition of
H2O2 formed an redish orangish solution, IIRC, not a deep red one. I guess the colour of the complex may vary depending on purity.
I was more interested in finding out the liquid it came in...
|
|
DrMario
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 332
Registered: 22-9-2014
Member Is Offline
Mood: Underpaid.
|
|
Quote: Originally posted by blogfast25 ![](images/xpblue/lastpost.gif) |
You'll probably have to fuse (dry it thoroughly first) it with sodium bisulphate, that's how insoluble and inert it is. It's reactivity does depend on
grade to grade.
My food grade Anatase TiO<sub>2</sub> doesn't even respond slightly to 200 C 98 % H2SO4.
Once dissolved (if you manage it), dilute the solution and add aluminium foil or zinc (in a test tube!). That causes any TiO<sup>2+</sup>
(titanyl cations, Ti(IV)) to be reduced to purple/deep blue Ti<sup>3+</sup>.
Adding hydrogen peroxide then causes a deep red peroxo titanium (IV) complex to form.
[Edited on 23-10-2014 by blogfast25] |
That's a nice experiment. I'd rather use concentrated sulfuric acid instead of melting sodium bisulfate. Melted sodium bisulfate seems a bit too
unstable. Maybe I'm just getting old, but boiling concentrated sulfuric acid is as far as I'm willing to go ![:D](./images/smilies/biggrin.gif)
[Edited on 24-10-2014 by DrMario]
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by DrMario ![](images/xpblue/lastpost.gif) | That's a nice experiment. I'd rather use concentrated phosphoric acid instead of melting sodium bisulfate. Melted sodium bisulfate seems a bit too
unstable. Maybe I'm just getting old, but boiling concentrated sulfuric acid is as far as I'm willing to go |
Phosphoric acid is unlikely to do it.
You can also fuse with NaOH or KOH: that forms titanate. With water that immediately hydrolyses to Ti(OH)4, which is much more responsive to acids
when freshly prepared.
Sodium bisulphate does decompose: it sheds SO3 and forms pyrosulphate. But it's not particularly dangerous.
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
A while ago I dissolved crude titanium dioxide (from scrap titanium) in molten sodium bisulfate as part of a purification. It takes time, and a lot of
heat, but it is feasible.
|
|
DrMario
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 332
Registered: 22-9-2014
Member Is Offline
Mood: Underpaid.
|
|
Quote: Originally posted by blogfast25 ![](images/xpblue/lastpost.gif) | Quote: Originally posted by DrMario ![](images/xpblue/lastpost.gif) | That's a nice experiment. I'd rather use concentrated phosphoric acid instead of melting sodium bisulfate. Melted sodium bisulfate seems a bit too
unstable. Maybe I'm just getting old, but boiling concentrated sulfuric acid is as far as I'm willing to go |
Phosphoric acid is unlikely to do it.
You can also fuse with NaOH or KOH: that forms titanate. With water that immediately hydrolyses to Ti(OH)4, which is much more responsive to acids
when freshly prepared.
Sodium bisulphate does decompose: it sheds SO3 and forms pyrosulphate. But it's not particularly dangerous. |
Phosphoric acid? I never mentioned phosphoric acid - where'd you get that??? ![:D](./images/smilies/biggrin.gif)
The reaction with fused hydroxides seems quite interesting, and one I'd feel reasonably safe to try. Thanks a bunch for the tip!
|
|
WGTR
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 971
Registered: 29-9-2013
Location: Online
Member Is Offline
Mood: Outline
|
|
Dissolving TiO2 into molten NaHSO4 is not a big deal, as long as you have either a fume hood, or a decent fan outdoors. The
bisulfate salt is available readily from hardware and pool supply stores. More importantly, it can be melted in a test tube without destroying the
tube. That is more than can be said for molten hydroxides, which will quickly dissolve glass.
As part of some solar cell experiments, I dissolved TiO2 into NaHSO4. Details are in this thread:
https://www.sciencemadness.org/whisper/viewthread.php?tid=27...
There is some SO3 that is given off, hence the need for ventilation. Also, an excess of bisulfate is needed, to ensure that the mixture
remains molten. A clear orange melt should result once all the TiO2 is dissolved.
|
|