Heterogeneous Catalysis
How to decide metal loading based on surface area of the catalyst support?
Is there any thump rule available to decide active metal loading based on surface area of support material?
Is there any thump rule like number of active site per nanometer square of support material? etc.,
Kindly disscuss indetail.
|
|
Nicodem
Super Moderator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4230
Registered: 28-12-2004
Member Is Offline
Mood: No Mood
|
|
The utmost we can do, is to discuss the lack of details. I can't speak for all of our members, but I for one cannot read your mind telepathically.
Your post makes no sense whatsoever, simply because you do not provide the most basic information that would make your question answerable. Please
read the posting guidelines in order to learn how to properly present your problem.
|
|
vinothan23
Harmless
Posts: 13
Registered: 8-7-2011
Member Is Offline
Mood: No Mood
|
|
Dear Nicodem,
Kindly apologize me. I will get back to you soon with more details.
Thanks.
|
|
vinothan23
Harmless
Posts: 13
Registered: 8-7-2011
Member Is Offline
Mood: No Mood
|
|
Catal Lett (2010) 138:215–223
in this above reference i read that
Dispersion of Cr={10^-18*NA}/{Surface area if AlF3*Mol.Wt AlF3}*(Cr/Al)
at the Cr/Al atomic ratio of 0.11 the dispersion of Cr is 12 atoms per nm2.
In another one patent US5281568, which states that loading of Zn based on working surface area of the catalyst.
If working SA is above 100 m2/gm Zn loading is 15-25% if it is 20-50 m2/gm Zn loading is 2-6% if it is less than 20 m2/gm Zn loading should be 0.5-1%.
So that i asked,
Is there any thump rule available to decide active metal loading based on surface area of support material?
Is there any thump rule like number of active site per nanometer square of support material?
How to decide metal loading based on surface area of the catalyst support?
|
|
Nicodem
Super Moderator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4230
Registered: 28-12-2004
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by vinothan23 ![](images/xpblue/lastpost.gif) | Is there any thump rule available to decide active metal loading based on surface area of support material?
Is there any thump rule like number of active site per nanometer square of support material?
How to decide metal loading based on surface area of the catalyst support?
|
You don't decide the catalyst loading just like that. You decide by measuring the catalyst activity. The catalyst loading for a process is a
compromise between economy, minimal turnover number and reaction kinetics. Surface area doesn't tell the activity of the catalyst, though it can be
expected that a catalyst with a higher specific surface area performs better than the same catalyst with a lower surface area, but there is no general
and fully linear correlation. Any such correlation would be reaction specific, just like catalysts are always mechanism specific.
You appear to generalize catalyst as if the type and reaction they catalyze is irrelevant which is obviously not the case. It is not possible to
describe complex systems with a single variable (they would not be called complex systems if this would be possible!).
…there is a human touch of the cultist “believer” in every theorist that he must struggle against as being
unworthy of the scientist. Some of the greatest men of science have publicly repudiated a theory which earlier they hotly defended. In this lies their
scientific temper, not in the scientific defense of the theory. - Weston La Barre (Ghost Dance, 1972)
Read the The ScienceMadness Guidelines!
|
|