Author: Subject: A small accident
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

shocked.gif posted on 11-12-2011 at 03:19
A small accident


Yesterday I had a funny day. I broke 3 vessels and one of them was containing hot sulfuric acid.
I needed just a small amount of conced H2SO4 for some testing so i was distilling 30% electrolyte, about 20 grams.

When i wasnt looking a piece of glass just shot out of the vessel (and later it cracked completely ofc)

I think that happened because the amount was too small and glass started expanding differently.

I think it might be useful to remind everybody that heating a nearly empty flask is as stupid as heating an empty one, im glad i didnt use my favourite glassware and there were only small amounts of acid, so nobody got hurt.

Heres a pic of Mr Coffee Still. RIP.

IMG_6814.JPG - 72kB
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 11-12-2011 at 04:21


Quote:
there were only small amounts of acid, so nobody got hurt.

This time . . . !
The moral of the story is; you need to drop your apparent cavalier attitude to safety!
I mean, heating H<sub>2</sub>SO<sub>4</sub> in any quantity in shit glass is begging for trouble!


View user's profile View All Posts By User
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

[*] posted on 11-12-2011 at 05:48


hey, dont insult him, he was pyrex :cool:

but yeah, my bad, i learned from it.
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 11-12-2011 at 07:44


Pyrex?
Genuine borosilicate doesn't fail by reconcentrating sulphuric acid!
Two lessons learned, perhaps . . .


View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 11-12-2011 at 08:18


Quote: Originally posted by hissingnoise  
Pyrex?
Genuine borosilicate doesn't fail by reconcentrating sulphuric acid!
Pyrex brand consumer glassware (like a Mr. Coffee) in the US is no longer borosilicate. Corning sold off US rights to the brand several years ago.
View user's profile View All Posts By User
starman
Hazard to Others
***




Posts: 318
Registered: 5-7-2008
Location: Western Australia
Member Is Offline

Mood: No Mood

[*] posted on 11-12-2011 at 09:25


You broke three pieces of glass.Same day,unrelated incidents?Perhaps you should reregister as 'Welcometothecasualtyward'.

[Edited on 11-12-2011 by starman]




Chemistry- The journey from the end of physics to the beginning of life.(starman)
View user's profile View All Posts By User
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

[*] posted on 14-12-2011 at 11:03


others were minor things. But i will consider that one :D
View user's profile View All Posts By User
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

[*] posted on 15-12-2011 at 07:33


Quote: Originally posted by hissingnoise  
Pyrex?
Genuine borosilicate doesn't fail by reconcentrating sulphuric acid!
Two lessons learned, perhaps . . .




And it didnt fail because of acid, i hope you understand that.
I have done that before.
View user's profile View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 15-12-2011 at 08:22


Quote:
And it didnt fail because of acid, i hope you understand that.

It failed because 'tempered' glass has a much higher C.O.T.E. than borosilicate glass!
Tempered glass is OK for heating water but sulphuric acid boils @ 337°C!


View user's profile View All Posts By User
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

[*] posted on 15-12-2011 at 08:39


But I was actually ''distilling'' water, right?
View user's profile View All Posts By User
Lambda-Eyde
National Hazard
****




Posts: 859
Registered: 20-11-2008
Location: Norway
Member Is Offline

Mood: Cleaved

[*] posted on 15-12-2011 at 08:46


I think accidents like these could be avoided in 95% of cases if people stopped dicking around and bought some real labware instead. A beaker can be had on eBay for a few dollars at most. Anyone can afford that, it's just a matter of priorities. Hobby chemistry doesn't have to involve using thousands of dollars on apparatus, equipment and chemicals, but it doesn't have to, and shouldn't have to revolve around improvising glassware. Using a few dollars on real glassware could save you an eye or your life...



This just in: 95,5 % of the world population lives outside the USA
You should really listen to ABBA
Please drop by our IRC channel: #sciencemadness @ irc.efnet.org
View user's profile View All Posts By User
Alastair
Hazard to Self
**




Posts: 59
Registered: 13-7-2011
Member Is Offline

Mood: Barely any solvent in my emulsion

[*] posted on 17-12-2011 at 06:07


Well i do have some glass, im just overly protective of it and i only use it when necessary. Just dont heat a nearly-empty vessel rapidly (yes it cracked at a place that had no contact with the liquid and i have sucessfully done it with a little larger amounts and more steady heating)

I presume that was a special day when god of chemistry took vacation from helping me :D
View user's profile View All Posts By User
MagicJigPipe
International Hazard
*****




Posts: 1554
Registered: 19-9-2007
Location: USA
Member Is Offline

Mood: Suspicious

[*] posted on 17-12-2011 at 20:33


Hmmmm... Just don't use non-borosilicate glass for heating anything but pure water. Ever. I learned that lesson the hard way (it only took one incident).

Trust me. That rule will never let you down.




"There must be no barriers to freedom of inquiry ... There is no place for dogma in science. The scientist is free, and must be free to ask any question, to doubt any assertion, to seek for any evidence, to correct any errors. ... We know that the only way to avoid error is to detect it and that the only way to detect it is to be free to inquire. And we know that as long as men are free to ask what they must, free to say what they think, free to think what they will, freedom can never be lost, and science can never regress." -J. Robert Oppenheimer
View user's profile View All Posts By User This user has MSN Messenger
jsc
Hazard to Self
**




Posts: 65
Registered: 16-3-2011
Member Is Offline

Mood: No Mood

[*] posted on 23-12-2011 at 12:20


Glass fractures are going to occur, even with real pyrex.

Whenever you work with heat, assume a breakage. Whenever you work with pressure/vacuum assume an explosion.

What is important is your containment system, and since you weren't hurt and no damage was done, your containment system worked. So you succeeded, good job.
View user's profile View All Posts By User
peach
Bon Vivant
*****




Posts: 1428
Registered: 14-11-2008
Member Is Offline

Mood: No Mood

[*] posted on 23-12-2011 at 14:36


Quote: Originally posted by Alastair  
But I was actually ''distilling'' water, right?


You'd be distilling up towards an azeotrope, which means the temperature will gradually rise from that of water towards that of azeotropic sulphuric acid as the remaining liquid becomes more and more concentrated and approaches it's own BP.

Once the temperatures start getting up towards 300 and 400 with borosilicate, you do need to consider letting it cool gently again; e.g. switch the heat off and leave it in place, as opposed to immediately removing or submerging it. It's hard to do with normal sized flasks and 200C, but borosilicate certainly can shatter due to thermal shock alone as the heating & cooling rates & masses involved increase; more so if the heating / cool is not uniformly applied. It's easier to shatter full glassware than it is empty, because there is can be a huge thermal mass on one side of the glass and another at a greatly different temperature on the other.

Regular kitchen ware, I've managed to shatter that attempting to make cups of tea in tumblers when I couldn't find a cup.

[Edited on 23-12-2011 by peach]




View user's profile View All Posts By User