Aluminium amalgam
Can someone help me with a good preparation of an aluminium amalgam because i'm sure i'm doing something wrong.
I was making an aluminium amalgam by a 2% solution of Mercury(ii)Nitrate in 200ml distilled water
I've cut 50gr aluminium foil in squares 2x2cm and put them in a beaker. Then i've put the solution over the aluminium and let it sit for a couple
minutes till hydrogen gas is vissible.
After a few minutes I've discarded the mercury solution and washed the alu foil with water. But when the water came in contact with the alu foil the
reaction started and almost all alu foil disolved.
What have I done wrong??
[Edited on 30-4-2014 by Hboomans]
|
|
leu
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 368
Registered: 13-10-2005
Member Is Offline
Mood: No Mood
|
|
Mercuric Nitrate is less soluble so it takes longer to get an amalgamation going than with mercuric chloride The mercuric ion can serve as a catalyst turning aluminum foil into aluminum hydroxide which produces hydrogen gas
during the reaction Mercuric Iodide is more soluble than mercuric nitrate and
thus might be more suited to your needs
Chemistry is our Covalent Bond
|
|
macckone
Dispenser of practical lab wisdom
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline
Mood: Electrical
|
|
Try using a more dilute solution of nitrate or a thicker grade of
aluminum foil with a larger quantity of foil.
It sounds like you are forming amalgam it is just too reactive.
|
|
GoldGuy
Harmless
Posts: 45
Registered: 24-11-2013
Location: Toronto, ON
Member Is Offline
Mood: Not sure if awake or in a dream where Im trying to fully awake.
|
|
You are using 5-10 times the amount of mercury necessary
|
|
CycloKnight
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 128
Registered: 4-8-2003
Member Is Offline
Mood: Still waiting for the emulsion to settle.
|
|
I've always had better success with sliced up aluminium pie tins. When thin aluminium foil has been consumed the surface area becomes very high and
the reaction can be very uncontrollable (depending on application). Thicker Al is also a lot less work to slice up (per gram) with some heavy duty
scissors.
|
|
Hboomans
Harmless
Posts: 6
Registered: 17-2-2014
Location: Netherlands
Member Is Offline
Mood: No Mood
|
|
I've done the amalgamation this time with the information you all gave me.
I've cut 30gr aluminium foil in sqaures about 2.5cm x 2.5cm and put them in a coffee grinder for a few seconds (because i've read this on the internet
about the coffee grinder)
I've placed the aluminium foil in a beaker and put 500ml h2o over the foil. The h2o i've made this first in a plastic bottle with 400mg mercury
nitrate, after about 10mins I saw that amalgamation has started so after that i've let it amalgamate for approx. another 10min.
After the amalgamation I discarded the h2o.
Now i've put the aluminium in my reaction vessel but nownothing happend, waited for 15min. still nothing happens. So I considerd putting another 400mg
mercury in the reaction vessel, after 2min. the reaction became so violent that it blows out of the condensor.
The foil I used i've measured it and it was .02mm so I've fold it once to get .04mm
What could have gone wrong??
I'm thinking of using aluminium barbeque trays the are .12mm thick. The reaction would be less violent, but the reaction would take longer. But does
anyone now how much longer the reaction will take place? Is there a way I can calculate that?
|
|
Nicodem
|
Thread Moved 3-5-2014 at 09:10 |
zed
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2281
Registered: 6-9-2008
Location: Great State of Jefferson, City of Portland
Member Is Offline
Mood: Semi-repentant Sith Lord
|
|
Umm. I had a buddy that used to run reductions with Aluminum Amalgam. Utilized a bathtub full of ice, and small, portion-wise additions of
ingredients to control the vigor of reaction.
That blowing out the condensor event....it isn't good. Commonly vents lots of hydrogen into the room, where it may mix with air and detonate. Not
healthy for living things.
|
|
leu
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 368
Registered: 13-10-2005
Member Is Offline
Mood: No Mood
|
|
The time taken for the reaction to run to completion depends on what substrate is being reduced The fact that the contents of the reaction vessel were ejected through the condenser says that the substrate that you
posted questions about in another thread recently results in a rather exothermic reaction which is what caused the new decorative markings on the
ceiling Your equipment isn't adequate for what you're trying to do in it, so
maybe you should study the subject more thoroughly before making another attempt at redecorating There's plenty of information about your queries available online already so there was really no need for this thread
to be posted