Engager - 18-9-2008 at 05:36
Today's research in energetic materials generates tons of new substances, but their properties are almost always
missed or incomplete. Sometimes all that you know about interesting compound is it's molecular structure (e.g bond chain and ordering). In order to
decide is it worth to spend time and resources on it's synthesis, abilty to predict energetic properties of new compound compound will be very
helpful. In general, prediction of properties is a hard work, but can be done even on simple home PC with use of common chemical software. I my post
i've tried to show it in most simple, general way, without deep going into special details. Much more detaled information about HEDM properties
prediction is avialable in journal articles and quantum chemistry books. Generaly, considering new energetic material we are most interested in four
main explosive properties: detonation velocity (this is proportional to substance density and heat of explosion), heat of explosion (this contributes
to explosion power), volume of explosion gasses (affects explosive power ant throwing ability) and sensitivity of explosive. All this, except
sensitivity can be predicted by means of some chemical calculations, without any experimental data required.
Essential software
First off all you will need to get some common chemical software, such as molecular structure modeling tools and
quantum chemistry package. Some additional visualization and file editing software is usefull as well. Here is a list of programs, witch i found
apropriate for our task.
1. Chemoffice Suite. This one is surely familiar to many people who use PC for
chemistry. This package contains some general compound modeling tools and some more advanced features, such as rectefication of structure using data
from build in compound structure database or simple optimization tools like MM2. Program can also serve as generator of input to further optimization
by quantum chemical software. You can review it here:
www.cambridgesoft.com/software/ChemOffice/.
2. PC Gamess quantum chemistry package. Surely other quantum chemical codes such as
Gaussian, or NWChem can also be used, but Gamess is best in terms of speed and is also free for academic use. PC Gamess is a freely available ab
initio and DFT computational chemistry program developed to offer high performance on Intel-compatible x86, AMD64, and EM64T processors. It was
initially based on the free GAMESS(US) program sources but extends its functionality in some important areas. The PC GAMESS project is maintained by
the staff of the Laboratory of Chemical Cybernetics at Moscow State University (MSU). The project coordinator and leading developer is Dr. Alex A.
Granovsky. You can download this package from official server here:
http://classic.chem.msu.su/gran/gamess/index.html.
3. In order do calculate substance crystal density using electron density maps
provided by PC Gamess, you will need special utility witch i've written specialy for this small article. If you are using Windows XP or later they
will run without any setup, if you use other outdated OS you will need VB Runtime Library installed in order to run it. Utility + source code +
article from Journal Of Hazardous Materials describing density prediction principle + examples of PC Gamess input & output + Chem3D files used for
calculation, can be downloaded in single archive here:
http://rapidshare.de/files/40492387/Density_Calc.rar.html
4. To make your work more comfortable and enjoy visualization on the fly you can
get some aditional tools such as Chemcraft (visualization tool for PC Gamess and 3D molecular structures), Ultraedit32 file editing tool, capable for
fast browsing and editing of big files and FAR file mannager for easy dos style file operations. Chemcraft is shareware, but is fully functional for
30 days after first run, there is also simplified free version avialable. You can get this program here:
http://www.chemcraftprog.com.
Then you got essential software, you can beging compound structure modeling. Properties witch we want to calculate
are only drop in the ocean, from listed software capabilities, so this programs can be very usefull in many other fields of numerical chemical
research.
Generation of initial compound structure
First of all, you must generate initial molecule structure. To do this launch ChemDraw (2D molecular structue
modeling tool from ChemOffice), create a new document and draw your molecule using toolbox at the left side of the screen. Don't worry if your
molecule looks asymmetrical or distorted, it can be easily rectified by pressing Clean Up Structure command in Structure menu (watch left picture
below). Then your molecule is assembled and rectified in Chemdraw you can transfer it to 3D modeling system of Chem3D. Select your molecule using
marquee tool and copy it to clipboard using copy button in edit menu. Now launch Chem3D, create new document and click paste in edit menu, your 2D
molecule will be pasted in 3D envouriment (watch middle picture below). To rectify structure in Chem3D and optimize it's steric energy you must use
Minimize Energy tool in MM2 menu, that will bring optimization options window, leave all parameters on default and click Run button - this will launch
MM2 steric energy minimization. Minimization takes some time, and you will see it's progress as atoms in your model will move arround, untile they
settle in energy minimum. Completion of minimization is signaled by word Ready in status bar. Note that optimizer will automatically add lone pairs to
several atoms, witch are shown as pink spheres. Rectified 3D structure got from initial one is presented on the right screenshot below:
After MM2 optimizaton your molecule is much closer to real one, but must be further optimized to get valid
structure. Final optimization and energy + properties prediction require job of quantum chemical software. Now you must export structure from Chem3D
to PC Gamess input file. Chem3D can export PC Gamess input files, however it can't set correct computation options in it, so you must create this file
by hand. Gamess input deck require set of all atom coordinates in your molecule, and assumes that molecule is better or less optimized, overvise
calculation may not converge. This is a bit of art in providing good initial structure, but one optimized by Chem3D usualy works well. To export file
with atom coordinates in format requred by PC Gamess, save file with structure from Chem3D, selecting "Gamess Input" file format. Now our initial
structure is complete and we can proceed to PC Gamess quantum chemical calculations.
Predicting heat of formation and optimizing molecular structure
As you may know, compound's heat of formation is related to structure of compound and is a measure of it's energy,
so positions of atoms in molecule relative to each other precisely defines structure energy and dirivated heat of formation value. This is not
completely precise, because we take our molecule as single one in free space (igeal gas), but in real crystaline cell molecule is always surrounded by
many others and this also affects structure energy. However energy difference done by placing molecule in crystalline cage (heat of vaporisation) is
usualy much lower in value then heat of formation, and can be completely skipped if we solve our problem in gas phase aproximation. Heat of formation
in solid or liquid state is always lower then one in gas phase, but heat of vaporisation is hard to be predicted due to extreme complexity of
calculations needed for it. You should realize that quantum chemestry calculations require a lot of computing power, and ammount of calculations rise
dramaticaly then using higher level of theory or growing number of atoms in molecule. In order to compute middle scale HEDM molecule in reasonable
time while still getting good quality output property values, we must select computation method very carefully. The most suitable method for our case
is semiemperical PM3, witch is fast and good in prediction of geometry and heats of formation. Now we must arrange input file for our job, this file
has general structure witch is shown on left picture below.
To give you any idea about what exactly listed parameters do, i give them a short description. First parameter group
($CONTRL) are most importans, as they control the job of PC Gamess program, and designate target of calculation. Our target is specified by keyword
"RUNTYP=OPTIMIZE" informing a program that we need to optimize molecule structure and get it's energy, keywords "COORD=CART" and "UNITS= ANGS" set
mode of input cordinates to cartesian 3D system using angstrom (10^-10 m) as units of lenth, keywords "SCFTYP=RHF" and "MAXIT=50" forces program to
use Restricted Hartree-Fock method to solve Schrodinger equation (core of quantum chemistry theory) for our molecular system and set iteration limiter
for it at 50 iterations. $GUESS and $BASIS groups determine choce of initial aproximate orbital primitives, witch will be used for numerical solution
of Schrodinger equation in our molecule, more detailed information about basis sets can be found in quantum chemistry literature. $STATPT group
controls stationary point search mode. Leave theese all untouched.
Next we have a $DATA group in witch our initial molecule is defined, by provided atom coordinates and core charges.
First line below $DATA contains job title witch will be displayed in output file, C1 key defines symetry of our molecule (C1 means no symetry and can
be used in any case), lines below contains atom names, core charges and coordinates. Don't worry we not need to calculate them by hand, they are
already saved to file by Chem3D program we used before, we just need to copy them to our input file. Contents of file saved by Chem3D is shown in
middle picture below. Then editing input file you must ensure that first character on all lines is space and there is line with keyword $END on end of
atom coordinate listing. Note that file saved by Chem3D also saves Lp atoms (lone pairs) witch are junk and must be discarded. Result of
copy&paste work is complete PC Gamess input file, witch is shown on right picture below:
Once input file is prepared it should be executed by PC Gamess, save input file to directrory where PC Gamess
executable is located with name "input", launch comand prompt, navigate to PC Gamess dirrectory and type "pcgamess >pm3.out", this will launch
calculations and save results to specified "pm3.out" file. Gamess calculations can take some time, so you can be interested in viewing progress at the
moment. To do that you can open "pm3.out" with FAR file viewer tool or by Chemcraft, in file viewer you can monitor calculation process in real time
and watch all current actions done by program, Chemcraft will show you 3D structure of your molecule at all optimization steps taken by PC Gamess. All
this shown on pictures below:
After execution is complete, you will get both, optimized molecular structure and corresponding heat of formation.
To get them open output file "pm3.out" and find line with statement "EQUILIBRIUM GEOMETRY LOCATED", below you will see set of atomic coordinates with
optimized molecule structure, corresponding heat of formation is slightly above this line, in the begining of final optimization iteration. You can
aslo visualize optimized (real) molecular structure by opening "pm3.out" by Chemcraft and selecting Optimized geometry in the step list. Results of
calculations viewed as mentioned above are shown on screenshots below:
As you can see in on the screenshot above, heat of formation of our structure in gas phase is calculated as 40.571
kcal/mol. If you want to convert this value to kJ/mol, you must multiply it by 4.1868, if you want heat of formation in kJ/kg value in kcal/mol must
be multiplied by (4.1868*1000/molar mass). Our optimized molecule structure can now be used for calculation of crystal density, we will find it in the
next step.
Predicting Crystal density
Density is very important for HEDM, because it dirrectly affects detonation velocity. That's why then looking for
new effective energetic compounds density is one of the main aims in search, and it very important to have ability to predict it at least aproximately
before spending time on synth of new compound. Modern theoretical work on computation of substane crystal density assumes that density is a function
of electron density in molecule and that volume of molecule in crystaline cell is proportional to volume of 3D region in witch electron density is
above 0.001 electrons per cubic bohr (bohr is unit based on hydrogen electron orbit radius). Electron density map can be computed by means of quantum
chemical software, so derived density value can also be determined. PC Gamess can produce electron density map, but it can't calculate volume of
reqired zone, this must be done by user or some other external program. Numericaly this task transforms in task of creating isosurface with 0.001
e/bohr3 density value, and calculation of it's inside volume, using electron density values mapped by PC Gamess in set of 3D mesh points. In order to
calculate requested volume we should split 3D mesh on cubes, each of those has some volume and electron density values at it's corners. It is clear
that if all this values are above 0.001 e/bohr3 our cube is inside isosurface and it's volume must be added to sum, otherwise if values at all corners
is below 0.001 e/bohr3 cube is outside isosurface and it's volume is discarded. If values at some corners of cube are bigger then 0.001 and lower then
0.001 at other - this means than isosurface intersects our test cube, cutting off some volume that must be added to sum, this volume can be
aproximated by deviding cube volume to 8 parts (number of cube corners) and multiplying this value by number of corners witch have value above 0.001
(e.g number of corners inside isosurface). Because electron density map produced by PC Gamess contains enumorous number of small cubes (millions),
volume sum obtainted then considering all this small cubes together will be very precise, but will also require some intense calculations, fortunately
we are not forced to do this by hand, this is PC live for. I've written small utility witch will do this operation using PC Gamess generated density
map, so our job is launch games electron mapping job and to open resulted output file by utility. Typical electron density mapping job input file is
shown on left picture below, lines with atomic cordinates are missed and should be filled with coordinates of our previous optimization run, witch we
done then predicting heat of formation. After copy&paste work we will get input file like one shown on right picture below:
![](http://img515.imageshack.us/img515/7083/image14vh3.th.jpg)
Before processing this new input file we must clean up PC Gamess directory from output generated from previous job,
otherwise this data could be overwritten and PC Gamess execution will terminate with warning about old output file existance. Make a new folder inside
PC Gamess one, and move old "input" and "punch" files to this folder. Now you can save new "input" file in PC Gamess folder, and execute it as in
previous run, using command prompt and typing "pcgamess >dens.out". I you examing new input file closely you will note that this time we used
another basis set, and used RUNTYP=ENERGY, theese are changed because PC Gamess can not generate electron density maps using PM3 and other
semiemperical basis sets, however to prevent computation of new molecular structure we used single point energy run, in witch structure of our
molecule will be preserved. After execution of our mapping job is completed we can open output files to watch obtained results, electron density map,
in witch we are interested is located in file called "punch" inside PC Gamess dirrectory. This file contains many other information, and our map is
located under $CUBE group and it's end is marked be $END keyword, as shown on screens below:
Now we can use produced electron density map to estimate crystal density of our compound. To do this just open it
with utility i've provided, type path to PUNCH file and click Load File button. Remember that utility recognizes only CHNO substances, and will fail
if substance contain other elements or if input file format is incorrect, so be sure to supply correct input file. Results of this operation are shown
on screenshot below:
![](http://img205.imageshack.us/img205/7265/image18as1.th.jpg)
As you can see on this screenshot, calculated crystal density of our compound is 1.896 g/cm3. However this value
must be corrected by multiplying it with 0.955 witch is correction factor for our basis set (PM3), introduced because calculated density produced by
this basis set is systematically higher then real. So for our compound we estimate density of 1.896*0.955 = 1.81 g/cm3, that is very close to
experimental value 1.82 g/cm3. If you want to visualize your resulting density map by Chemcraft, or to use it for input in some other programs, you
can convert it to CUB file format. This is easily done by copying all data between $CUBE and corresponding $END group in "punch" file and saving it a
new file with .CUB extention. This file can be visualized by Chemcraft program, density isosurface drawn by chemcraft and part of this exported .CUB
file are shown on the screens below:
Predicting heat of explosion and explosion gas volume
Heat of explosion determines, how much energy is released then our substance detonate. As you may know heat
generated from rection is sum of formation heats of explosion products, subtracted by heat of formation of initial compound. To calculate heat of
explosion we must assume some detonation equation, revealing products of detonation process and their proportions against each other. Generaly
detonation can be assumed as simple burning process, in witch carbon inside explosive compound is oxidized to CO2, hydrogen to H2O and nitrogen to N2,
by using oxygen contained inside explosive molecule. But how can we be then oxygen contained in molecule present in larger or smaller ammount then
required to get only this products? Then there is too many oxygen in molecule we must assume that excess oxygen is released in free state (O2), if
there is not enough oxygen for full oxidation situation is bit more complicated and we must take to account atom oxidation "priority". Hydrogen gets
oxidized on first place, and oxygen will be used to form H2O until all hydrogen atoms will be oxidized, and only then oxygen will be used to oxidize
carbon backbone, free hydrogen is released in explosion only if there is not enougth oxygen in initial molecule to fully oxidize is (for example in
HN3 explosion). Carbon is first oxidized to carbon monixide CO, CO2 will form only if there is enough oxygen remaining, to form CO and CO2 mixture,
and only CO2 if oxygen content is enough for full oxidation. Free carbon can be released only then not enough oxygen remaining to convert all carbon
atoms to CO, and will be released in mixture with CO if oxygen content of explosive is too low. This model is reasonably simpified, but can be used
for getting some usefull information about properties of explosive. Four our case (RDX, C3N6H6O6) we can assume following decomposition
equation:
C3N6H6O6 = 3H2O + 3CO + 3N2
Heat of formation of initial explosive compound is already known from calculation and to get heat of explosion we
need to know heats of formation of explosion products. These can be calculated in same way by using PM3 method in PC Gamess, and are precalculated as
(also in kcal/mol): CO = -19,74453 ; H2O = -53,42649 ; CO2 = -85,03881 ; N2 = 17,56604 ; O2 = -21,42657. Using this value and molecular mass of our
compound we can calculate heat of explosion in several units:
Hexpl (kcal/mol) = [3*(-53.42) + 3*(-19.74) + 3*(17.56)] - [40.57] = -166.8 - 40.57=
-207,37 kkal/mol = -868,216716 kJ/mol = -3908,949 kJ/kg
Minus sign means that heat is released (exotermic reaction). This value is lower then experimental (-5297 kJ/kG) by
about 1400 kJ/kg. Our result is inaccurate because experimental heat is taken using solid compound (and we assumed gas state reaction) and also
because heat of formation depends from temperature whitch is not same as room temperature used then computing our heat of formation values, simplified
detonation equation also takes part in this inaccuracy. While resulted value is not very precise, it still very usefull, because it can be used to
compare different energetic molecules with each other, taking to account the fact that real heats of explosion have same proportions to each other as
calculated ones if compound is of the same class. For example, we know experimental and calculated heats of explosion for compound A, and for compound
B of same class we know only calculated heat of explosion, we can use this data to get real heat of explosion for compound B: Acalc/Bcalc =
Areal/Breal ; Breal = Areal*Bcalc/Acalc.
Detonation equation witch we assumed above can also be used to calculate explosion gas volume, that is important
factor contributing to power of our explosive. As you can see in decomposition equation above 1 mol of our compound (RDX) generates 9 mol of gaseous
products. Taking to account the fact that 1 mol of any ideal gas at room temperature is 22.4 liters, we can calculate volume of explosion gases:
Vgas = 22.4 * 9 = 201.6 l/mol = (1000/222.11) * 201.6 = 907 l/kg
Calculated value is very close to experimental (908 l/kg), so volume of explosion products can be predicted quite
accurately, if explosion detonation equation is composed correctly. You may heard about Trauzl bomb test for explosives, it measures expansion power
of explosion gases, and depends only from heat of explosion and explosion gas volume. This value can aslo be derivated using parameters we calculated
above, but has no much interest for us.
In next post i will show how to calculate detonation velocities at different densities using calculated data above.
497 - 18-9-2008 at 17:02
This is very interesting stuff indeed. I can't wait to see more.
I have recently downloaded Hyperchem 7.5. I have not play with it much so far, I don't know how its capabilities compare to the above stated programs
but it looks like it does some similar functions. Do you know anything about it?
Engager - 19-9-2008 at 13:57
Predicting Velocity of detonation
Detonation velocity is one of the main factors, determining power of explosive. The detonation velocity is the rate
of propagation of a detonation in an explosive; if the density of the explosive is at its maximum value, and if the explosive is charged into columns
which are considerably wider than the critical diameter, the detonation velocity is a characteristic of each individual explosive and is not
influenced by external factors. It decreases with decreasing density of packing in the column. The standard hydrodynamic theory used for computing VOD
of an explosive is concerned only with the amount of energy liberated and the nature of end products, and is independent of chemical reactions. The
density, heat of formation and atomic composition can be integrated into an empirical formula for predicting performance of a proposed
explosive.
There are many different relations describing dependence of detonation velocity from explosive constitution, and
they use different parameters witch are used for velocity estimation, however most common are explosive constitution, heat of formation, oxygen
balance and of course density. Formulas have different degree in accuracy and often give good estimations for some class of explosive compounds, while
giving prediction with less accuracy for another compound classes. In our case we are interested in ones, witch give reasonably good predictions for
any compound class, and use computationaly available parameters. It should be noted that in many formulas detonation velocity is much more dependent
on constitution of explosive, then from heat of formation, and inaccurate heats of formation got from calculations (gas phase value, not taking to
account crystalline energy effects) are perfectly suitable for prediction of detonation velocity. In reverse to heat of formation, density greatly
affects detonation velocity and is one of the main factors controlling it, good thing is that computed densities are precise enough to perform good
estimations of detonation velocity.
Now, I will show you how to use two different sets of empirical formulas to estimate detonation velocity and
detonation pressure. First formula, having more simple nature, was described by Aisenshtadt in Russian explosive material journal, it can be used to
estimate detonation velocity from heat of formation, explosive constitution and oxygen balance:
At this formula Hf is heat of formation in kcal/mol, Mw is a molecular mass of explosive compound in g/mol, p is
explosive density in g/cm3, D1.6 is detonation velocity in km/sec at 1.6 g/cm3 and Dp is detonation velocity at target density (p) it is also in
km/sec. Use of this formula is pretty straight forward, just use your explosive formula, predicted heat of formation and select density you want to
use in calculation, but don’t forget to convert your heat of formation into kcal/mol, before substitution to formula. Example results for our
calculated molecule (RDX) are shown below:
C3H6O6N6 ; Hf= 40.571 kcal/mol ; r = 1.8 g/cm3 ; B = ((3 + 6 + 6 + 6)/222.117)*1000 = 94.544 ; OB =
|16(6-6-3)/222.117|*100 = 21.610 ; Qv = - |(40.571 + 0.3(6+6+6))/222.117| * 1000 = -206.964 ; M = 3 ; D1.6 = (0.73*94.544 – 0.24*21.610 +
0.0073*206.964)^0.5 = 8.083 km/sec ; D1.8 = 8.083 + 3(1.8-1.6) = 8.683 km/sec.
Note, that in formula above B is factor dependent from substance constitution, OB is form of oxygen balance, and Qv
is approximate heat of explosion. All this are multiplied by coefficients got by fitting experimental data for many explosive compounds, and all this
values are finally united then completing detonation velocity. This is a philosophy of empirical formulas – select properties witch as we think
are determining value being estimated, and then fit experimental data to get coefficients for estimated value formula. Formula above can also be used
for mixtures of explosives, in this case explosive formula and heat of formation must be substituted by corresponding average values for explosive
mixture. As you can see calculated detonation velocity is pretty close to experimental (8.750 km/sec), error is only 0.75%. Divergence can vary for
different classed of compounds, but formula usually give satisfactory results.
To give an alternative to Aisenshtadt formula, i will also show usage of formulas proposed by M.H. Keshavarz
(References: Propellants, Explosives, Pyrotechnics 30 (2005), No. 2 ; Predicting the Detonation Velocity of CHNO Explosives by a Simple Method ; pp
105-108 and Journal of Hazardous Materials A119 (2005) 25–29 ; Simple determination of performance of explosives without using any experimental
data). This formula uses calculated gas phase heat of formation (calculated in same way as we done – by PM3 method) of explosive compound
instead of experimental one, and volume of explosion gasses derivated from estimated explosive detonation equation. Method assumes that all heat
generated by explosion is used to heat explosion products, that allows to estimate explosion temperature witch is then used in pair with explosion gas
volume and density to estimate detonation velocity. Estimation of explosion temperature is bit of art in numerical way, and requires some math
operations or numerical analysis. To estimate explosion we must use heat balance for our process, but we can’t simply use standard heats of
formation of explosion products as we done then estimating heat of explosion, method requires to take account to temperature dependence of heat of
formation in explosion products. Heat of formation is function of temperature, exact equation for this dependence can be obtained from isobaric heat
capacity vs temperature dependency, this one is usually approximated in polynomial form as shown on illustration below. Heat of formation vs
temperature function is obtained by integration of this dependency, as shown below:
![](http://img178.imageshack.us/img178/9549/fla2sk3.jpg)
Cp is heat capacity at constant pressure ; Hf are heats of formation ; T is temperature ; Nj is number of moles of
product j in detonation equation ; A,B,C,D,E,F are constants for each individual compound obtained by fitting experimental heat capacity data.
Equation at the bottom of illustration above is heat balance equation, showing that all heat released by explosion is used entirely to heat explosion
product (adiabatic explosion), since explosion process is extremely fast, adiabatic assumption is pretty much accurate. To solve heat balance
equation we can use simple numerical method called bisection.
Bisection method is a root-finding algorithm which repeatedly divides an interval in half and then selects the
subinterval in which a root exists. Suppose we want to solve the equation f(x) = 0. Given two points a and b such that f(a) and f(b) have opposite
signs, we know by the intermediate value theorem that f must have at least one root in the interval [a, b] as long as f is continuous on this
interval. The bisection method divides the interval in two by computing c = (a+b) / 2. There are now two possibilities: either f(a) and f(c) have
opposite signs, or f(c) and f(b) have opposite signs. The bisection algorithm is then applied recursively to the sub-interval where the sign change
occurs (watch illustration below).
![](http://img510.imageshack.us/img510/2928/fla3mm1.jpg)
To solve our heat balance, first we must transform our heat balance equation to form suitable for bisection f(x)=0,
next we reasonably assume that explosion temperature lies somewhere between room temperature and some high temperature for example 6000K. Now we are
ready to solve our problem, we just need to get coefficients from explosion equation (Nj’s), coefficients got by fitting experimental heat
capacity (A, B, C, D, E, F) and heat of formation of our explosive witch we calculated before. Be aware that these experimental coefficients are
calculated to fit heat equation then T/1000 is used instead of simple temperature value, so to get correct results you must place T/1000 in place of T
in equation below.
C3N6H6O6 = 3H2O + 3CO + 3N2
For example i will show single calculation of f(T) at T=600K, so you can see how data listed above is working in our
equation. Be careful, heat balance root finding takes a lot of simple calculations, be sure to make no errors in signs, numbers and choose proper
temperature intervals in table, or you will get completely confusing results. Here is an example, i’ve mentioned:
Root bracketing is now straight forward, bisection method is stable and usually converges quite fast. Method is the
same as in bisection method description, but f(x) is replaced with our function f(T), results are shown in table below. As you can see method
converged to temperature about 3731K witch is our explosion temperature. Amount of calculations is too big to by hand, that’s why i’ve
written utility for calculation of detonation parameters, PC must pay by fair work for money you spent on it.
![](http://img178.imageshack.us/img178/4562/flatable2ca8.jpg)
Now, then temperature of explosion and volume of explosive gasses is known, we can simply calculate corresponding
detonation velocity, by means of simple formula shown below. In formula (r) is density at witch detonation velocity is being predicted (g/cm3), Texp
is temperature of explosion in K found in calculations above, (n) is a amount of gas generated by 1 gram of explosive (simple sum of mole numbers of
explosion products in right side of detonation equation, divided by molecular weight of our explosive, value in mol/g), resulting detonation velocity
will be in km/sec.
![](http://img510.imageshack.us/img510/6132/fla6cl2.jpg)
Substitution of our data (T=3731K, p = 1.8 g/cm3; n = 9/222.11 mol/g) we get detonation velocity of 8899 m/sec,
experimental value at 1.8 g/cm3 is 8750 m/sec. So found detonation velocity is slightly overestimated, error is 1.67%, so accuracy is also very good,
especialy taking to account the fact that when we started we known absolutely nothing about our compound! Formula works well on many classes of
explosive, but requires some intense calculations.
Now we have predicted velocity witch is quite precise, but one may also want to predict detonation pressure,
fortunately it’s very easy as it can be predicted using only heat of formation and explosive composition, as shown in another M.H Keshavarz
article. Formula for calculation of detonation pressure is shown below:
Here Hf is explosive heat of formation (we already calculated it way before), r is density in g/cm3, Mw is molecular
mass of our explosive, resulted detonation pressure will be in kbar. Using data for our explosive (a=3, b=6, c=6, d=6, Hf=169.86 kJ/mol, r=1.8 g/cm3)
we can calculate detonation pressure for our explosive, witch is 414 kbar (experimental is 341 kbar) with 18% error, however with no surprise due to
gas phase calculated heat of formation, instead of crystalline experimental one. On experimental heat of formation formula gives much more precise
result (355 kbar calculated vs 341 kbar measured).
In total, from zero knowledge starting point we have predicted: heat of formation, crystal density, volume of
explosion gasses, detonation temperature, detonation pressure, detonation velocity. Of course there are many other estimation methods, but this ones
are simple and can be made at home. For convenience i have written small utility witch calculates estimated parameters using methods described above
and in references mentioned. Utility requires VB runtime libraries, but if you use windows XP it should run without any setup. Utility with the source
code + references for this article in small archive file are attached to this post, screenshot is shown below:
That’s all for now, any opinions & comments about this work will be gladly
appreciated. If you found some bugs in utilities i provided please report them to me by personal message. Questions on property calculation topic can
be asked in this topic.
[Edited on 20-9-2008 by Engager]
[Edited on 20-9-2008 by Engager]
Attachment: Detonation2.rar (345kB)
This file has been downloaded 1473 times
Engager - 19-9-2008 at 14:04
Quote: |
Originally posted by 497
This is very interesting stuff indeed. I can't wait to see more.
I have recently downloaded Hyperchem 7.5. I have not play with it much so far, I don't know how its capabilities compare to the above stated programs
but it looks like it does some similar functions. Do you know anything about it? |
Thanks for your inerest, it's good to see that i'm not alone here. Regretably i haven't got Hyperchem to watch for it's capabilities, but if you need
any of software i've mentioned in my post i can upload it.
[Edited on 20-9-2008 by Engager]
497 - 20-9-2008 at 01:09
That is a pretty awesome little program! And an amazing feat of mathematics too. It works perfectly so far.
I think a useful addition would be a table of actual values (det vel, gas vol, etc) of various explosives. That would give one something to compare
their outputs to see accuracy, and just to get a practical idea of its power. I know that information is scattered around, just I've never seen it
condensed into a single table.
Also having some kind of scale to get an idea of the extrapolated test values (sand crush, lead block expansion, etc.) based on the output values
from the program would be useful.
A heat of formation calculator would be really nice too.
Another idea: similar programs except for fuel-air detonations, thermobaric enhanced explosives, metalized explosives, etc. I suppose it might be
harder to find computational methods for those though.
I would love it if you could upload those programs if its not too much trouble.
Here are a couple resources I ran into recently. They have some interesting computational and expiremental research and going on at Caltech. The
military site has a lot of nice old scanned in stuff from the 80s, on all kinds of subjects.
http://www.galcit.caltech.edu/EDL/publications/references/ed...
http://www.dtic.mil/dtic/search/tr/index.html
I for one think you are doing a great service for all of us interested in energetics. Keep up the good work!
Engager - 20-9-2008 at 07:52
I've uploaded software i've metioned to: http://rapidshare.com/files/146893683/Essentials.rar.html
Package is ~100 Mb size and contains the following stuff: Chemoffice8 & Serial ; PC Gamess 7.1 with samples, help files, and some additional
extentions ; Chemcraft 2.63 + keygen ; UltraEdit32 File Editor + crack ; Density and Det.Velocity utilities for this thread with source codes on VB6 ;
files used for calculations in topic above ; references on computational methods used.
Far file manager can be downloaded for free here: http://www.farmanager.com/files/FarManager170.exe
Formatik - 20-9-2008 at 10:26
Thanks for the programs. It's also possible to estimate the relative strength equivalent, which results most resemble the trauzl test. They are
formulas most likely built on deriatives, and likley most applicable to CHNO compounds, but I've seen favorable results even with some inorganics (see
below). Among one of these formulas is one seen here: http://www.fas.org/man/dod-101/navy/docs/es310/chemstry/chem... Here are some estimates: Method 1 is the one in the site above. For the second
method I'd have to find it again.
compound.............Method1......Method2.....Actual lead block (%TNT)
urea nitrate..............91.................44................90
EtONO2...................122...............147..............140
trinitromethane.........84................120..............137
HNAB.........................--.................133...............122
MeONO2..................242..............197..............203
NH4NO3....................--..................61...............60
NH4ClO4....................--..................51...............65
isoPrONO2.................56..................42..............56
N2H4.HClO4...............--...................120............121
TEGDN.......................92.................79...............106
Hexanitrobiphenyl.....111...............114..............120
DEGDN......................136................133.............136
TeNMe........................46..................69...............21
There is a small table of detonation velocities here: http://www.sciencemadness.org/talk/viewthread.php?tid=3416
For heat of formation values, see here: http://cobweb.ecn.purdue.edu/~propulsi/propulsion/comb/prope...
Microtek - 25-9-2008 at 10:23
@ Engager:
I have tried your method with the supplied programs and am very impressed with the amount of work that you have done.
I have a few comments however; I tried it with TNT and got a density of ca 1.76 (after the 0.955 correction factor). Needless to say, this gave quite
a high VOD. Do you know if this method gives poor predictions for nitroaromatics, or if maybe I made an error?
Secondly (and more importantly) I tried with HNIW but couldn't get the PM3 calculation to converge. It gave an error message saying that it made too
many iterations, so I increased the MAXIT parameter to 1000 which didn't resolve the issue.
Could you try to run the program for HNIW and report if you can make it reach a conclusion? I am doing some work with HNIW and related compounds at
the moment, so it would be quite valuable with a predictive tool.
Engager - 25-9-2008 at 15:14
Quote: |
Originally posted by Microtek
@ Engager:
I have tried your method with the supplied programs and am very impressed with the amount of work that you have done.
I have a few comments however; I tried it with TNT and got a density of ca 1.76 (after the 0.955 correction factor). Needless to say, this gave quite
a high VOD. Do you know if this method gives poor predictions for nitroaromatics, or if maybe I made an error?
Secondly (and more importantly) I tried with HNIW but couldn't get the PM3 calculation to converge. It gave an error message saying that it made too
many iterations, so I increased the MAXIT parameter to 1000 which didn't resolve the issue.
Could you try to run the program for HNIW and report if you can make it reach a conclusion? I am doing some work with HNIW and related compounds at
the moment, so it would be quite valuable with a predictive tool. |
Well, 0.955 factor works very fine on caged nitramines and tetrazoles, witch i've tried to calculate. Benzene aromatics like TNT can have different
value because PM3 computaion method produces results of different quality on differented molecule classes. This is not a error of calculation by my
utilities. In order to get good correction factor for benzene nitroaromatics, take a set of molecules with known density, compute them to get
calculated densities without 0.955 correction and select correction factor witch suits computed vs experimental data.
Your problem with HNIW is based on fact that you used incorrect starting struture for input of Gamess, remember it will never converge unless
structure you give is correct and at least slightly optimized by implementing MM2 in Chem3D as i described. HNIW computation works very fine for me, i
got density 2.043 vs 2.04 experimental with usual 0.955 (2.141 * 0.955 = 2.044 g/cm3) correction. Input files for PC Gamess jobs, and results of
successful jobs on HNIW using method i've described in my article are placed in archive here:
http://rapidshare.com/files/148417525/CL-20.rar.html
To give you any idea how good initial Chem3D - MM2 structure looks like, watch the picture below. Left structure is produced by Chem3D+MM2 and right
one is optimized by gamess and is taken from converged PC Gamess PM3 run.
[Edited on 26-9-2008 by Engager]
Microtek - 26-9-2008 at 02:10
OK I tried it again and I noticed that the nitrogroups that I draw in chemoffice look somewhat different from yours. Mine are drawn with a delocalized
doublebond while yours look like N-O single bonds. Also, if I use the MM2 operation after attaching the NO2's, then the nitro groups are changed to
sp3 hybridization rather than sp2 (which is how they start out).
Anyway, by running the MM2 operation on just the skeleton without any NO2 groups and then attaching these afterwards gave me the correct result. I
suspect I'm not using chemoffice quite correctly.
Engager - 27-9-2008 at 12:15
Due to the report of Microtec i found error in detonation velocity utility, problem is in Visual Basic representation of numbers, this is now fixed,
and work correctly then HNIW data is entered (Formula - C 6 H 6 N 12 O 12 ; Hf - 451,12 kJ/mol ; Density - 2,04 g/cc), new version is attached to this
post.
[Edited on 27-9-2008 by Engager]
Attachment: Detonation3.rar (27kB)
This file has been downloaded 1242 times
The_Davster - 28-9-2008 at 18:02
Some silly questions:
How do I use the chemoffice keygen? My virus scanner picks up keygen.nfo because whenever I click it it attempts to contact the internet....
I have no idea how to install the PCGamess7.1...where is the setup.exe file?
Microtek - 28-9-2008 at 23:18
I couldn't get chemoffice activated either, so I found another version on avaxhome. As for PCGAMESS, it is ready to go when unpacked; no installation
required.
chief - 29-9-2008 at 13:23
Maybe it's possible to predict some of the properties of the explosive, as long as the bondings and reaction-products are known, thereby the
temperature, pressure, molecular velocity etc ..
But I'm not gonna believe properties of materials could be predicted (today) unless somebody shows that he can deliberately invent eg. new
superconducting materials, alloys with specifyable thermal hardening properties or something else. Science is far from that today.
The method also seems to be limited to the organic chemistry, also the empirical formulae are adjusted on the known properties of the materials: No
wonder, if some of the results comply with the lead-block test ... .
But anyhow, a useful thing to have is a structural database: From there on you can investigate and go onto adventure. Unfortunately I never found any
rapidshare-link to a version of the CCSD (CAmbridge crystal structure database, http://www.ccdc.cam.ac.uk/), maybe someone could help with that ?
Engager - 29-9-2008 at 22:42
Quote: |
Originally posted by The_Davster
Some silly questions:
How do I use the chemoffice keygen? My virus scanner picks up keygen.nfo because whenever I click it it attempts to contact the internet....
I have no idea how to install the PCGamess7.1...where is the setup.exe file? |
This is funny =) nfo files are not executables but are simple text files opened by notepad, in one of theese following numbers vere given for
Chemoffice registration: serial: 7654321 reg-key: VLPG-CG5O-5K22-VKVK-RF . Microtek told me that negative heats of formation can not be entered in
detonation utility, this is now fixed, fixed version is attached to this post. And one more thing if some admin reads this post, please remove
attached previous versions of this file, so people can download only fixed one.
Attachment: Detonation4.rar (27kB)
This file has been downloaded 1263 times
PROJECTING AN ESTIMATE OF PERFORMANCE
franklyn - 29-9-2008 at 22:46
I believe old tricks are the best especially if there is no apparent improvement with newer methods.
To estimate a hypothetical explosive's performance one need only know it's structure , be able to
do arithmetic , and have a calculator that does square roots.
- - here you must enter fractional exponents within parenthesis ^ ( 1/2 )
http://www.math.sc.edu/cgi-bin/sumcgi/calculator.pl
- - this does not accept fractional exponents, one must do power and root separately
http://firstyear.chem.usyd.edu.au/calculators/chemical_calcu...
The two references immediately following and previously cited by me outline exactly how to proceed.
Honestly I don't know why I bother to post references when apparently no one takes notice
http://www.sciencemadness.org/talk/viewthread.php?tid=7518&a...
Estimation of the Density of Organic Explosives from Their Structural Formulas
http://fas.org/sgp/othergov/doe/lanl/lib-www/la-pubs/0032140...
also available in the Science Madness library
http://www.sciencemadness.org/lanl2_a/lib-www/la-pubs/003214...
It's not necessary to re-invent the wheel if it gets you to the same place
the method is very simply stated by example on pages 3 , 4 , 18
and in an earlier post
http://www.sciencemadness.org/talk/viewthread.php?tid=1222#p...
A Simple Method for Calculating Detonation Properties of C-H-N-O Explosives
http://www.dtic.mil/cgi-bin/GetTRDoc?AD=AD661483&Locatio...
the relevant formulas and procedure is concisely expressed on pages 9 , 13 , 25
- - Another reprint with sequels is attached at the bottom of this post - -
- - the same procedure and formulas are on pages 26 , 28 , 33
A demonstration by steps is in the following post in this thread
If anyone has any quarrel with the preceding , know that the method has also been cited
by the luminary Gerald Hurst. That's good enough for me.
http://yarchive.net/explosives/detonation_pressure.html
Out of academic interest only , the following linked from my second cited post above
and made available again by engager in an attachment to this current thread here.
http://www.sciencemadness.org/talk/viewthread.php?tid=7518&a...
Simple determination of performance of explosives without using any experimental data
http://www.keepmyfile.com/download/90d8582111582
Password = references forum password
- This is essentially the same paper in a different journal -
Predicting the Detonation Velocity of CHNO Explosives by a Simple Method
http://www.keepmyfile.com/download/0d5a8f2192372
Password = references forum password
Predicting Heats of Formation of Energetic Materials Using Quantum Mechanical Calculations
http://www.arl.army.mil/arlreports/2001/ARL-RP-15.pdf
.
Attachment: Calc Det Prop of CHNO HE.djvu (681kB)
This file has been downloaded 1284 times
HOW TO APPRAISE PERFORMANCE OF HYPOTHETICAL - C H N O - EXPLOSIVE
franklyn - 29-9-2008 at 23:13
- In 4 easy steps
The following example demonstrates the steps to estimate how one can project the
probable performance of an explosive.
Pg 33 Organic Chemistry of Explosives - Agrawal
Addition and condensation reactions employing nitroform or its methylol derivative,
2,2,2-trinitroethanol, have been used to synthesize a huge number of compounds
containing the trinitromethyl group. Such compounds often have a very favorable
oxygen balance which contributes to explosive performance. However, compounds
containing the trinitromethyl group often exhibit an unacceptably high sensitivity to
shock and impact. [ Only testing of the actual compound can determine if it merits
further consideration ]
I have been reviewing literature on a notion I have for applying nitroform as a functional
group. The idea is to attach four trinitromethyl groups to pentaerythrite. I had planned
to post how this hypothetical molecule might be synthesized and possible approaches
to producing the precursors. Nitroalkanes are derived from this trinitromethyl group by
the well established and long ago documented method of nitro-dehalogenation. The
pathway indicated would use a tetra(halo)pentaerythrite with a metal nitroformate
salt to form Pentaerythrite Tetranitroformate - PETNF
This yields 20 mols of gas and has a slight positive oxygen balance.
. . . . . . . . C[ CH2.C( NO2 )3 ]4 => 9 CO2 + 4 H2O + 6 N2 + O2
1 )
The first thing then is to draw a structure
Arguslab a feature rich , superb molecular modeling program is what I use to resolve
structure , just click the " pliers " icon in the tool bar until converged. This entire part
can be skipped , it only serves as a visual aid and to confirm that the object can exist.
Free download here -> http://www.arguslab.com
The 3D Argus *.agl file of PETNF is in the zip file attached below.
[url]
[/url]
2 )
To derive a value for the density I have applied the method of H. H. Cady cited above in
LA-7760-MS , http://www.sciencemadness.org/lanl2_a/lib-www/la-pubs/003214...
Estimation of the Density of Organic Explosives from Their Structural Formulas
To establish the density , the molecule must be dismantled into component pieces
for which the volume is known. Density is then derived by adding up all the pieces
and dividing the molar weight by the sum of these volumes.
Tables of these, are given in the cited reference along with their values.
C[ CH2.C( NO2 )3 ]4 , breaks up into the following functional groups or free radicals.
Group. . . . . . . . . . . . . . Carbon . . . . . . . Methylene . . . . . . . N i t r o
. . . . . . . . . . . . . . . . . . . . . . C . . . . . . . . . . . C H 2 . . . . . . . . . . N O 2
Volume of each . . . . . . .3.3 . . . . . . . . . . .10.16 . . . . . . . . . . 17.02
How many of each . . . .X 5 . . . . . . . . . . . . .X 4 . . . . . . . . . . . X 1 2
Totals for each . . . . . . 16.5 . . . . . . . . . . 40.69 . . . . . . . . . 204.24
Table II ( C - ? ) + ( ? - NO2 ) => C - NO2. . . Added correc. .0.54 . . .Total of Volumes = 2 6 7 .9 1
= ( V )
One also needs to estimate the packing factor or coefficient ( k ) figured by formula 4
on page 18. k = 0.7686 - 0.1280 (a) where (a) is
the fraction of
( number of hydrogen atoms bonded to carbon ) divided by ( total atoms in molecule )
in our case 8 / 53 = 0.01932 and so , k = 0.7686 - 0.1280( 0.01932 ) = 0.7493
Density ( ρ ) is weight divided by volume , according to formula 6 page 18
factor ( k ) is included thus ( mol weight )( k
) divided by ( V )
The molar weight of the substance is 668.23 and so times 0.7493
and divided by 2 6 7 .9 1 comes to ρ = 1.87 gm /cm³
* Note : Density of a crystal does not necessarily reflect actual loading density of a charge
comparing to ( k ) values of related known explosives we may assess this further
explosive . . . .Hexanitroethane . . . . PETN . . .
. ( average )
calculated . . . . . . 0.77 . . . . . . . . . . . . 0.73 . . . . . . 0.75 . .
observed . . . . . . . 0.68 . . . . . . . . . . . . 0.76 . . . . . . 0.72 . .
3 )
It's now necessary to determine the heat of formation of the compound to be analyzed.
Enthalpy changes for reactions can be obtained by simply subtracting the heats of
formation of the reactants from the heats of formation of the products. Thus if the
heats of formation of reactants that form the compound are known , the ∆Hf
Heat of formation of the compound will also be known.
It is important to know that for the purposes of determining enthalpies , the reaction
pathway need not be realizable in practice , and merely serves to ascertain the
∆Hf Heat of formation. http://pages.prodigy.net/anderhan/ch11thermo.pdf
For simplicity the hypothetical condensation of 1 mol of Pentaerythritol with
4 mols Trinitromethane as a base-acid esterfication is assumed.
The following values in kilocalories per mol are applied for thermodynamic calculations
- 57.8 for H2O ( g ), - 68.3 for H2O ( lg ) , - 94 for CO2 , - 220 for Pentaerythritol , - 16.25 (liq) Trinitromethane
Sources of thermodynamic properties
http://cobweb.ecn.purdue.edu/~propulsi/propulsion/comb/prope...
http://webbook.nist.gov/chemistry
http://www.update.uu.se/~jolkkonen/pdf/CRC_TD.pdf
http://www.arl.army.mil/arlreports/2001/ARL-RP-15.pdf
In accepting the condensation of Pentaerythritol with Nitroform , you see the
advantage for calculation of showing only water as a co-product of synthesis
. . . . C(CH2OH)4 + 4 HC(NO2)3 => C[ CH2.C( NO2 )3 ]4 + 4 H2O
Heats of formation of the reactants is subtracted from that of the products to
infer the ∆Hf Heat of formation : 4 H2O ( lq )
is - 273.2 , minus ( - 220 + 4 (- 16.3 )
Arithmetically subtracting a negative is the same as adding a positive so ∆Hf is + 11.8 kcal /mol
Now the heat of explosion can be calculated simply
∆Hf Heat of formation of Pentaerythrite
Tetranitroform is subtracted from the detonation
products to infer the ∆He Heat of explosion:
C9H8(NO2)12 -> 9 CO2 + 4 H2O + 6 N2 + O2
(9 CO2 is - 846) + (4 H2O ( g ) is - 231.2) + (N2 & O2 are zero) minus (+ 11.8) = - 1089 kcal /mol
Dividing the ∆He Heat of explosion of 1 mol of
the compound by it's molar weight , - 1089 / 668.23
obtains ∆He Heat of explosion = - 1 6 3 0 Kcal per kilogram of compound
This will be assigned to the constant Q in step 4
4 )
To estimate the Detonation pressure generated and Velocity of Detonation ,
I have applied the method of M.J. Kamlett, S.J. Jacobs outlined in
The Journal of Chemical Physics , vol 48 , num 1 , cited and also attached above
http://www.dtic.mil/cgi-bin/GetTRDoc?AD=AD661483&Locatio...
A Simple method for Calculating Detonation Properties of C-H-N-O Explosives
Also in LLNL Handbook of Explosives section 8.1.2 Estimation on page 8.9
what follows does not referer to this LLNL Handbook , but to the Journal of Chem. Phy.
The formulas presented amount to generalized shortcut calculations for determining
values that according to its author will typically occur around 2 % of real values.
M is grams of gas per mol of gas , equation 14 page 27
N is mols of gas per gram , equation 13 page 27
P is detonation pressure expressed in kilobars ( 1 Bar = 1 atmosphere )
ρ density given as grams per cubic centimeter 1.87
Q is ∆He Heat of explosion in calories per gram 1 6 3 0
So this can be easily understood ,
the constants that count each type of atom , given in the article as a , b , c , d
in the formulas for M and N , are changed here to the atom each represents a = C (Carbon)
b = H (Hydrogen) , c = N (Nitrogen) , d = O (Oxygen)
M = . . .56 N - 88 O - 8 H . . . = . . . 56( 12 ) - 88( 24 ) - 8( 8 ) . . . = 35.6
. . . . . . . . 2 N + 2 O + H . . . . . . . . . . 2( 12 ) + 2( 24 ) + ( 8 )
N = ... 2 N + 2 O + H . . . . . . . . . . = . . . .2( 12 ) + 2( 24 ) + ( 8 ) . . . . . . . . . . . . . .≈ 0.03
. . . . 48 C + 4 H + 56 N + 64 O . . . . . . 48( 9 ) + 4( 8 ) + 56( 12 ) + 64(
24 )
The formulas given for M and N intend to acount
for what carbon remains unreacted
in explosives with negative oxygen balance. This does not apply in this case and the
value of M X N = G = calculates to 1.068 , indicating a corrective subtraction of - 6 %
specified on the bottom of page 33 and 35
We now have all the necessary values to calculate this : ( N √ M √ Q )
( Q ( 1 6 3 0 ) is substituteded here without
regard for sign )
( * Note this expression is given as ф ( phi ) in the article ) . . . ( 0.03 ( 5.97 ) ( 40.37 ) ) = 7.23
Detonation pressure = P = 15.58 ρ ² ( N
√ M √ Q )
. . . . . . . . . . . . . . . . . . . . . . . . . 15.58 ( 1.87 ) ² ( 7.23 ) = 3 9 4
kilobars
minus - 24 , 6% correction factor comes to 3 7 0 kilobars
This is comparable to HMX in performance.
Velocity of Detonation = VOD = 1.01 ( 1 + 1.3 ρ
) √ ( N √M √Q)
. . . . . . . . . . . . . . . . .1.01 ( 1 + 1.3 ( 1.87 ) ) √ ( 7.23 ) = 9.318 millimeters per microsecond
multiplied by one million to obtain meters per second ,
minus - 559 , 6% correction factor comes to ≈ 8 7 6 0 Meters / sec
.
If the download here won't work for you try this link instead
http://www.badongo.com/file/11550199
Attachment: Pentaerythitol tetranitroformate.zip (6kB)
This file has been downloaded 1224 times
Microtek - 29-9-2008 at 23:36
@ Franklyn
In step 3 where you calculate heat of formation, you would also need to know the temperature change in the reaction; if the hypothetical condensation
reaction is endo- or exothermic you would under- or overestimate the heat of formation respectively.
franklyn - 29-9-2008 at 23:54
Quote: |
Originally posted by Microtek
@ Franklyn
In step 3 where you calculate heat of formation, you would also need to know the temperature change in the reaction; if the hypothetical condensation
reaction is endo- or exothermic you would under- or overestimate the heat of formation respectively. |
Yes point taken , but then I'm not a chemist.
Applicable enthalpies can be found in references I'm sure.
But that depth of involvement in thermodynamics is beyond me.
It appears to be endothermic as related compounds.
so won't be too far off.
.
Calculating blast radius
franklyn - 30-9-2008 at 00:20
Now that you have designed the mother of all energetic compounds,
what can be done with It , and how would you know it ?
That is a very complicated question
Blast radius is not a line in the sand where the explosion stops. The effect of
the explosion proceeds outward to an arbitrary distance of your choosing. If
you are at some distance away and the sound damages your hearing, does
this figure into your definition of "Blast Radius" ? All explosions are qualitatively
different. The hyperbaric effect of fuel air ordinance is not the same as the
underwater explosion of Torpex.
Upon detonation, a military high explosive expands the metal housing of the
ordinance to 1.5 times it's original diameter before breaking into fragments.
Typically 40 % of the weight is the explosive, the remaining 60 % is the casing.
Of the total energy liberated, half may be used up expanding the casing prior to
rupture and imparting velocity to the fragments. The remainder of the available
energy is expended in compression of the surrounding air forming an expanding
shock front that moves out supersonically. After a short distance the speed and
pressure of this front decreases much faster than the decrease in speed of the
casing fragments. This is due to the fragments having constant cross sectional
area and aerodynamic drag, while the surface area of the expanding shock front
increases as a function of the surface area of a sphere, Area = 4 ∏ ( r *squared )
( where r is the distance from the center of explosion to the shock front ).
distributing its energy at a decreasing intensity.
There are two measurements of the quality of the explosion, its peak pressure
and it's impulse or duration , this being the area under the graphed positive
pressure curve , which decreases by the reciprocal of the radius 1/ r
from the center of explosion. Peak pressure is carried by the shock front, an
extreme form of sound wave that transmits only energy. The pressure impulse
follows with the cyclonic surge of displaced air. Shock front and impulse are
disassociated and act independently. The momentum of the gas moving outward
behind the shock front expands it's volume until the pressure decreases below
atmospheric producing a rarefaction and reversal of the motion back toward the
center of explosion , while the shock front continues it's outward travel.
Remember that the energy is dissipated kinetically as a percussive wave into
the surroundings. See Pg 4 here ->
http://www.dsto.defence.gov.au/publications/2641/DSTO-TN-052...
[url]
[/url]
One can begin by finding the volume of gas produced by the explosive.
Consider the glycol dinitrate reaction : C2H4(NO3)2 -> 2CO2 + 2H20 + N2
the explosion of one mole of glycol dinitrate produces in the gaseous state:
2 moles of CO2; 2 moles of H2O; One mole of N2. A molar volume of gas at 0 °C
and atmospheric pressure occupies 22.4 liters. Since each mole produces one
molar volume of gas, a mole of glycol dinitrate produces 2 + 2 + 1 = 5
molar volumes of gas; and these molar volumes at 0 °C and atmospheric
pressure form an actual volume of 5 × 22.4 = 112 liters of gas. ( Note that the
products H2O and CO2 are in their gaseous form.) Based on this it can be seen
that the volume of the products of explosion can be predicted for any quantity
of an explosive.
Further, by employing Charle's Law for perfect gases, the volume of the products
of explosion may also be calculated for any given temperature. This law states
that at a constant pressure a perfect gas expands 1/273.15 of its volume at 0 °C,
for each degree Celsius of rise in temperature.
For example, at 15 °C the molar volume of an ideal gas is equal to :
The expansion by the increase in temperature ( 15 °C X 1 /273.15 X 22.414 )
plus + the original volume at 0 °C ( 22.414 ) = 23.645 liters per mole.
Thus, at 15 °C the volume of gas produced by the explosive decomposition of
one mole of glycol dinitrate becomes : V = (23.64 ltr./mol)(5 mol) = 118.2 ltr.
for the final adiabatically expanded quiescent volume. For a shallow underwater
explosion this defines the volume of the bubble that will be formed.
* Note :
For the radius volume V must be expressed in cubic meters M, there are 1000 liters
in a cubic meter so , 118.2 / 1000 , V = .1182 cubic meters
Setting this amount equal to the volume of a sphere : 4 ∏ ( r *cubed ) divided by 3
and solving for the radius : r = cube root of ( 3 V divided by 4 ∏ )
r = 30 cm , ( a ball of gas two feet across )
this gives you a naive working value for blast radius without regard to the proximity
with the ground and resulting Mach reflection. Nor the kinetic force of the shock
front and fragmentation. This later effect of fragmentation can be approximately
estimated by finding the cube root of the weight of explosive in kilograms, and
multiplying this by 130, giving the radius for the inclusion area in meters. Most,
but not all, of the fragments hurled out from an explosion will lie within this area.
Pieces moving with an azimuthal elevation between 45 and 50 degrees to the
horizontal will attain the greatest range, and a few of these will reach beyond
the inclusion area.
Without the use of calculus estimates for explosive effects are only approximate.
None of the above takes into account the energy transfer to the surrounding air.
An estimate for this can be made by applying the ideal gas law PV = nRT
which is an equation of state that describes the behavior of gases derived from
the combined gas laws used above. Pressure in atmospheres ( P ) times
volume in liters ( V ) equals = the number of moles ( n ) times
this constant .0821 ( R ) times the temperature in degrees Kelvin ( T ) ,
( which is degrees Celsius plus 273.15 )
This equation is much simpler to use than the sequence of steps applied in the
example above. Solving for the volume V = nRT/ P ,
V = ( 5 moles )(.0821 )( 15 °C + 273.15 ) / 1 atmosphere
is 118.2 Liters just as before.
The ideal gas law is really an energy equation which defines the potential
energy in a gas , the left hand side of PV = nRT
gives the value in Liter atmosphere ( L atm ) a unit of energy used for gases.
41.3106 Liter atmosphere is equal to one Kilogram Calorie.
To obtain useful and practical information about the explosion requires knowing
the initial temperature of the explosion which is itself usually only inferred by
calculation. One does however know the quantity of explosive used and it's known
caloric energy value. In the example used above, Glycol,dinitrate is rated at
approximately 1500 Kilogram Calories per Kilogram. Multiplying this value by the
amount of Nitroglycol used expressed in kilograms ( one mole ) .152 Kg., gives us
228 Kcal/ Kg. Using what we know and have established , 228 Kcal/ Kg ,
times 41.3106 Liter atmosphere , is 9419 Liter atmosphere.
9419 Liter atmosphere has a double meaning in that it can be seen as one liter
at 9419 atmospheres, as well as 9419 liters at one atmosphere. This is because
equation PV = nRT is in the form representing Boyle's law for gases PV = (constant)
This law states that for constant temperature and quantity ( moles ) of gas, it's
pressure and volume vary inversely to each other thus : ( P1 )( V1 ) = ( P2 )( V2 )
Solving for V2 = ( P1 V2 )/ P2 , since ( P1 V1 ) is 9419 , by dividing 9419 Liter atms
by a different amount of pressure ( P2 ) the volume for any arbitrarily chosen
pressure can be easily determined and with it the radius at that pressure.
Since any small elevation of ambient pressure will cause damage, the value of
one atmosphere will be used.
To calculate a blast radius, just as before, the volume is first converted into
cubic meters by dividing 9419 by 1000. Thus 9.42 cubic meters is set equal to the
volume of a sphere and solving for the radius, gives the value of 1.31 meter, a ball
more than 8 1/2 ft !
The difference between this and the 2 foot size given before, represents the
energy transmitted as a blast wave into the surroundings. Rarefaction will have
already occurred at this size having collapsed the detonation products into something
close to a 2 foot ball of gas, and the blast wave will have slowed and decayed into a
sound wave moving out at the speed of sound.
The difference of one meter , between being 1.31 meters away , and just 30 cm.
from a third of a pound of detonated Nitroglycol with fragmentation, is the difference
between an open casket , and a closed casket funeral.
For very large detonations the margin is not so clear. For example, 100 Kg of AN + Al
is 2350 Kcal/Kg times 100 = 235000 , divided by 228 in the previous example
is 1031 times greater. The radius enlarges to 13.23 meters, or 10 times the size.
At this range you may be killed by the concussion just from the shock front.
Significant energy is still carried by the shock front out beyond the vicinity of the blast.
It's magnitude depends on the size of the initial explosion.
Note also that the zone affected and at risk for fragmentation damage
extends out 2/5 of a mile.
To review :
Determine the caloric value of the amount of explosive used , multiply this by
41.3106 to obtain V in Liter atmospheres, divide by 1000 to convert this to
cubic Meter atmospheres and solve r = cube root of ( 3 V divided by 4 ∏ )
Simplified to : ( HE wt.)( HE cal/kg )(.009862 )^1/3
As an excercise , calculate a blast radius for the BLU82 depicted here ->
http://en.wikipedia.org/wiki/BLU-82
and post your results. I am curious to see who needs to ask
how to calculate a blast radius , if all that's required is pushing a pencil.
There is a very useful calculator online that will express all the sperical values
here -> http://www.cleavebooks.co.uk/scol/calsph.htm
Further reference
http://www.fas.org/man/dod-101/navy/docs/fun/part12.htm
___________________________________________________
For F.A.E explosions _
Based on the known properties of flammable substances and explosives, it is
possible to use conservative assumptions and calculate the maximum distance
at which an overpressure or heat effect of concern can be detected. Distances
for potential impacts could be derived using the following calculation method
[described in Flammable Gases and Liquids and Their Hazards]:
D = C(nE)1/3
where D is the distance in meters to a 1 psi overpressure; C is a constant for
damages associated with 1 psi overpressures or 0.15, n is a yield factor of the
vapor cloud explosion derived from the mechanical yield of the combustion and is
assumed to be 10 percent (or 0.1) and E is the energy content of the explosive
part of the cloud in joules. E can be calculated from the mass m of substance in
kilograms times the heat of combustion Qc in joules per kilogram as follows:
E = m Qc
Combining these two equations gives:
D = 0.15 x (0.1 m Qc)1/3
.
chief - 30-9-2008 at 09:34
Putting data into black-box-programs is _not_ science ! Besides commercial and half-commarcial software is a NO anyhow. A self-respecting thinker
writes his own code and maybe uses some some tools, eg. for visualization ... .
Why not do the real science: Where are the quantum-mechanics ?? In the qantum-mechanical software ??? Better if the formulae are here, so anyone can
follow the physics/chemistry in detail !
Then it also becomes quite interesting, and more satisfying than to handle (not so) _cool_ software-packages ....
After all: A human is not a trained monkey ...
What one really needs:
==> structural database (eg. CCSD: http://www.ccdc.cam.ac.uk/ , also ICSD: http://icsdweb.fiz-karlsruhe.de/)
==> knowledge
==> some ODE-solver-routines etc. for the language of choice might be helpful
==> a good visualization-tool: eg. http://www.geomview.org/
After all: The whole "prediction" here seems to come mainly from
==> calculating the pressure from
--> the initial density of the chemical bondings
--> the heat generated (specific to the bondings, heat gives temperature, that gives pressure)
--> the molar amount of gas produced (which is heated to the temperature(calculated from the heat))
It's simple physics, so no reason to demean oneself to black-box-operating any software, except if the aim is to impress some old grandmothers and the
like ...
But anyhow it's interesting stuff above, but a real man does the calculatons himself !!
Microtek - 30-9-2008 at 12:34
OK, so could you do a write-up of the quantum-chemical calculations to predict the density of RDX? Just so that those of us who don't feel so at home
with quantum mechanics can see how it is done....
franklyn - 30-9-2008 at 20:14
Recall that forum member enhzflep began this thread here
http://www.sciencemadness.org/talk/viewthread.php?tid=5712&a...
High Explosives Calculator
and submitted this H.E.Calc v 1.0
forum member not also provided a utility to average mixtures
forum member sylla provided code to run a program
the references posted by forum member Axt are expired now
This reference posted by enhzflep there is a good start for anyone
wanting to improve the art.
http://gltrs.grc.nasa.gov/reports/1994/RP-1311.pdf
.
chief - 1-10-2008 at 02:04
RDX-density-prediction:
First:
==> You just need the structure of the RDX;
==> this you get from the above mentioned CCSD
You _cannot_ relyably predict the structure, because science is just not far enough for that ! All you can do is take assumptions,
==> like how specific atoms arrange their bondings _usually_ ,
==> but this works best for compounds that are far from the unstability of explosive compounds, eg. with proteins you can toy around using the
3D-puzzle-software and try to find a place where some other molecule of the same shape might match.
Often this is sold afterwards the other way around, like: We calculated ... and experiment gave the proof; but the truth is: First by empirical means
all the compounds are tested, and then the calculations are done ... .
All that can be done quantum-mechanically is to be found in the average textbook about it, like:
==> What wave-functions do exist on what boundary-conditions
==> This does not go beyond the most simple compounds, like NH3 or H2O, and even there loads of parallel theories do exist
Only _few_ scientists have an idea of how to some-sort-of predict properties of a compound, and those are also the ones who _successfuly_ make a
breakthrough on some field, like eg. high-temperature-superconductors. Even Those few men (no women amongst them to my knowledge) do _lots_ of
experimenting, before they find a material, and then they find just one sort of a compound, and do some substitutions on it (similar elements on
similar places), like eg. the YBaCU-superconductors.
That why I say: Only thing that one can do is
==> get a quantum-mechanical textbook (maybe some internet-ressource exists too)
==> _and_ et a structural database, sor organic compounds the CCSD,
==> for inorganic structures the ICSD
==> those databases cost $$$$, no web-downloads known to me
==>but the average student might gain access via the university (data may be exported as csv-files; table-structure like mysql or other known
databases, ca then be re-imported into any other database)
Now that you have the nice CCSD or ICSD (each with around 100000 compounds stored in it) you just lookup the structure, get the measurements of the
unit-cell, count the atoms within it and calculate the density. But thats not prediction.
If anyone were able to relieably predict the properties of compounds, then he just could let the computer run and get himself a secretary to do the
patenting-stuff. Intuition one must have for predicting chemical properties.
Today still whole departments of universitary institutions are thrown at even simple tasks, and oftentimes find nothing, like eg. solar-cell-materials
and the like.
Then there of course do exist some packages, like the (GA)MESS, but these are just loads of theories put into code, just for checking around what
might be. If it's true or false always the experiment decides, it's like lottery for even the most of the professionals, and computers didn't change
that in the last 20 years (but are very useful for more simple tasks, like from the pressure calculate the dynamics of the pressure-wave-expansion,
using ode-solvers and the like, _where_ sufficiently simple laws hold).
Thats why I say: The best thing one can do is to get structural data, write himself some code, get knowledge and see how far it gets ! This way at
least the theory may be checked upon real existing evidence, the structural data within the databases !! These are what to get started from !!!
Engager - 1-10-2008 at 07:26
You are talking not about computing, if you can get experimental structure you can also get experimental properties. Stuff i was posted above can give
ZERO KNOWLEDGE aproximations, surely theese are not precise, but they are good then comparing theoretical structures and getting crude values to
decide is there any reasons to spend money and time to produce proposed compounds. If you are a wordeater and neglect everything computed, you may
continue to do so and stop loading topic with your complains. Your conversation style shows that you are not a scientist or not educated one, clever
people always try to watch at problem from all sides, trying to separate good seeds from any aproach, while stupid complacent people only complain and
neglect everething that not suits their oppinion.
[Edited on 1-10-2008 by Engager]
chief - 1-10-2008 at 07:52
I bet you can't name a single compound that was found by means of your method, right ?
The formulae are adjusted by the properties of the known materials, and that's why those known materials give good results. The adjustment-procedure
is known as "fitting", excessively used everywhere up from engineering (can be done eg. with "gnuplot").
The software-links you named lead to commercial-software-selling-sites, that's suspicious by itself. (Mine too, but for my links there are no
substitutes). ...
Besides: As long as you call me "stupid complacent people" I might as well think of you as an "software-kewl"
Next week we predict explosive power on the x-box-game-console ..
[Edited on 1-10-2008 by chief]
Engager - 1-10-2008 at 08:17
Well, now i see who you are, i have no further comments, good luck with self-enjoyment.
chief - 1-10-2008 at 10:51
Yeah, Thanks ! While I stay critical and don't fool myself I at least can grow on the problem ...
franklyn - 1-10-2008 at 20:58
C O R R E C T I O N
The expression shown for determining a value for M
as well as the value for M shown , are both in error .
The formula for M as seen in the attached Journal of Chem. Phy. article
shows the middle term , 88 O , of the numerator having a minus sign, that's wrong !
The original Naval Orinance Laboratory ( NOL ) citation depicts this correctly
as positive ( + ) as does the LLLNL Handbook on pg 8.9.
As I had previously done the calculations and saved the work , I just transcribed
that and copied the expressions ( the erroneous one ) from the text. There is
great peril in doing this and not performing cursory checks. I addittionally added ,
instead of subtracting , the rightmost term , 8 H . The correct figure for M is , 34.
M = . . .56 N + 88 O - 8 H . . . = . . . 56( 12 ) + 88( 24 ) - 8( 8 ) . . . = 34
. . . . . . . . 2 N + 2 O + H . . . . . . . . . . 2( 12 ) + 2( 24 ) + ( 8 )
N = ... 2 N + 2 O + H . . . . . . . . . . = . . . .2( 12 ) + 2( 24 ) + ( 8 ) . . . . . . . . . . . . . .≈ 0.03
. . . . 48 C + 4 H + 56 N + 64 O . . . . . . 48( 9 ) + 4( 8 ) + 56( 12 ) + 64(
24 )
The formulas given for M and N intend to acount
for what carbon remains unreacted
in explosives with negative oxygen balance. This does not apply in this case and the
value of M X N = G = calculates to 1.02 , indicating a corrective subtraction of - 6 %
specified on the bottom of page 33 and 35
We now have all the necessary values to calculate this : ( N √ M √ Q )
( Q ( 1 6 3 0 ) is substituteded here without
regard for sign )
( * Note this expression is given as ф ( phi ) in the article ) . . . ( 0.03 ( 5.83 ) ( 40.37 ) ) = 7.06
Detonation pressure = P = 15.58 ρ ² ( N
√ M √ Q )
. . . . . . . . . . . . . . . . . . . . . . . . . 15.58 ( 1.87 ) ² ( 7.06 ) = 3 8 5
kilobars
minus - 24 , 6% correction factor comes to 3 6 2 kilobars
This is comparable to HMX in performance.
Velocity of Detonation = VOD = 1.01 ( 1 + 1.3 ρ
) √ ( N √M √Q)
. . . . . . . . . . . . . . . . .1.01 ( 1 + 1.3 ( 1.87 ) ) √ ( 7.06 ) = 9.208 millimeters per microsecond
multiplied by one million to obtain meters per second ,
minus - 552 , 6% correction factor comes to ≈ 8 6 5 6 Meters / sec
.
franklyn - 1-10-2008 at 21:15
Using the method of H. H. Cady cited above in LA-7760-MS
on 2,4,6-Tris(trinitromethyl)-1,3,5-triazine , depicted below
Molar . . . . . . . . . . . . . . . Molar
Weight . . . . . . . . . . . . . Volume
46.01 . . . . . . . . . . . . . . 17.02 = NO2
. . . . . . . . . . . . . . . . . . . . +0.54 add correc
. . . . . . . . . . . . . . . . . . . .17.56
. . X 3 . . . . . . . . . . . . . . . . X 3
138.03 . . . . . . . . . . . . . 52.68
+ 12.01 . . . . . . . . . . . . . +3.3 carbon
150.04 . . . . . . . . . . . . . .55.98 trinitromethyl
. . . X 3 . . . . . . . . . . . . . .. . X 3
450.12 . . . . . . . . . . . . .167.94
+ 78.05 . . . . . . . . . . . .+33.73 triazine
_528.7 .X .7 6 8 6 .÷ . 201.67 = 2.013 gm /cc
Density estimate is 5.4 % over actual = 1.91
As no hydrogen is contained , K = .7 6 8 6
![](http://upload.wikimedia.org/wikipedia/commons/3/30/TTNMTZ.png)
The question is raised that
Comparative analysis of this methodology can be made on similar known compounds
with different oxygen balance , such as
2,4,6-Tris( trinitromethyl )-1,3,5-triazine,
which has excess oxygen with no hydrogen , C3 N3 [C( NO2 )3 ]3 => 6 CO2 + 6 N2 + 3 O2
and produces 15 mols of gas per mol
and 2,4,6-Tris( trinitroethyl )-1,3,5-triazine
with oxygen deficiency and hydrogen , C3 N3 [CH2.C( NO2 )3 ]3 => 6 CO2 + 3 CO + 3 H2O + 6 N2
yet produces 18 mols of gas per mol
Wikipedia quotes density to be 1.91 for the tri-trinitromethyl triazine
http://en.wikipedia.org/wiki/2,4,6-Tris(trinitromethyl)-1,3,...
This is the paper cited on the wiki page - that link is dead.
http://www.sciencedirect.com/science?_ob=ArticleURL&_udi...
Synthesis of 2,4,6-Tris(trinitromethyl)-1,3,5-triazine
Mendeleev Communications; Volume 5 (1995), Number 1, Pages 17-18
http://www.rsc.org/publishing/journals/RC/article.asp?doi=rc...
Nitro derivatives of 1,3,5-triazine: synthesis and properties
Russ. Chem. Rev., 2003, 72, pages 279 - 287
http://www.springerlink.com/content/f04565p1q5h37r21
Synthesis of N-trinitroethyl derivatives of linear and heterocyclic nitrogen-containing compounds
Russian Chemical Bulletin, Volume 54, Number 5 / May, 2005, Pages 1346-1349
This is an excerpt of this paper above - C L I C K the image to view it larger in another window
[img]http://resources.metapress.com/pdf-preview.axd?code=f04565p1q5h37r21&size=large[/img]
.
franklyn - 2-10-2008 at 14:38
Rapid and Accurate Estimation of Densities of Room Temperature Ionic Liquids and Salts
Ye, C.; Shreeve, J. M.
J. Phys. Chem. A.; (Article); 2007; 111(8); 1456-1461.
http://pubs.acs.org/cgi-bin/abstract.cgi/jpcafh/2007/111/i08...
Supporting information ( addendum to article ) - free download
Contains useful data
http://pubs.acs.org/subscribe/journals/jpcafh/suppinfo/jp066...
_______________________________________________
Ionic Liquids & Microwave Activation in Organic Reactions
herkules.oulu.fi/isbn9789514287190/isbn9789514287190.pdf
On pg 91 - condensation of pentaerythritol with acetic acid.
Trinitromethane could serve as well but only if it can be done
at lower temperature for safety sake.
A related article
Microwave in Organic Chemistry
stoltz.caltech.edu/litmtg/2003/yeeman-lit-6_11_03.pdf
.
franklyn - 21-1-2009 at 18:44
Quote: |
Originally posted by franklyn
Quote: | Originally posted by Microtek
@ Franklyn
In step 3 where you calculate heat of formation, you would also need to know the temperature change in the reaction; if the hypothetical condensation
reaction is endo- or exothermic you would under- or overestimate the heat of formation respectively. |
Yes point taken , but then I'm not a chemist.
Applicable enthalpies can be found in references I'm sure.
But that depth of involvement in thermodynamics is beyond me.
It appears to be endothermic as related compounds.
so won't be too far off. |
It occurs to me that an expedient way to assess the missing enthalpy of reaction ,
is by comparing the average bond energy of disassociated bonds of the reactants
to the formed bonds of the products.
Using this source > http://www.cem.msu.edu/~reusch/OrgPage/bndenrgy.htm
Thus :
BOND . . . . . C - O . . . H - C . . .
-> . . C - C . . . . O - H
ENERGY . . . 85.5 . . . . 99 . . . .
.-> . . . 83 . . . . . . 111
TOTALS . . . . . . . .184.5 . . . . . . . . . . . . . . . . 194
The difference is 9. 5 Kcal
multiplied by the 4 reaction sites, comes to 38 Kcal / mol reaction enthalpy
If the value for products is less than for reactants then the difference is endothermic
If the value is greater for the products , as in this case , the difference is exothermic
The adjustment is made simply by increasing or decreasing the amount given for the
formation : ∆Hf is + 11.8 kcal /mol is therefore decreased to - 26.2 kcal /mol
As the heat of explosion was overstated by ~ 3.6 % , { 38 / ( 1089 - 38 ) = 38 / 1051 }
all subsequent calculations are similarly diminished.
.
sylla - 13-2-2009 at 02:21
Very nice! Really.
A few years ago, I have developped a very same program and model on my own. It's quite nice to see that I used techniques very close to yours.
Unfortunately, I never achieved to make algorithms to predict densities so the program was incomplete (my goal was to make a standalone model, mostly
for educative purposes).
But there are still possibilities to improve your program by a few tricks that can achieve quite nice results actually. (I used to have less than 2%
error on the VOD of RDX, for example, which is so low that it falls in the experimental error range).
Depending on the oxygen balance of the explosive you can use the Kistiakowsky-Wilson or modified Kistiakowsky-Wilson rules. It is also possible to add
new rules to cover more exotic heteroatoms. For example :
Halogen : X --> HX
Sulfur : S --> SO2
Metals (Na, K etc..) : M --> M2CO3
Metals (Ca, etc...) : M --> MO
But what does actually make the difference is the accuracy in decomposition product. Estimmating the products of reaction using the
Kistiakowsky-Wilson rules is actually a very bad, rough, approximation. However, it is possible to build really nice estimmations using equilibria
(considering there are fast enough to take place in explosion). For example you have :
CO2 + H2 <--> CO + H2O
2 CO <--> C + CO2 (*** important because of the loss of gaz ***)
CO + H2 <--> C + H2O (*** important because of the loss of gaz ***)
.5 N2 + CO2 <--> CO + NO
Again, these equilibria will depend on the temperature but so does the heat released and therefore the temperature! This kind of retroaction loop can
be treated through numerical computations again.
1. First Compute the product using the "simple" rules.
2. Compute the heat of reaction and temperature.
3. Compute the current equilibria values for the given temperature.
4. Apply the equilibria to the reaction products (which is another story yet...)
5. Recompute the heat of reaction and temperature.
6. If the difference between the "old" temperature and the "new" one is greater than a given epsilon (about 10°C), go back to step 3.
This is computationaly more expensive than applying the dichotomial algorithm on the temperature profile. But it worth the trial and can be done in a
few ms on a modern computer.
Again, there is yet another possibility to improve the program. By approximating a compound of various explosive as being linear/ideal (ie: there is
no modification by blending two explosive with density d1 and d2, the resulting density being computed directly from d1 and d2 alone), it is possible
to compute the best ratio of two (or more) components.
For example, if we would mix gasoline and air the program would have detected that the most powerful concentration ratio would not have been the
stoichimetric one but, let's say, something that has x% more gasoline. When I worked on my software, years ago, I managed to compute the "best"
(theoretical) ratio for mix such as H2/O2 (which is not the stoichiometric ratio again!) or NH4NO3/TATP and so on. What was actually missing in my
work was that I had too little experimental data to compare with the theoretical one... Though the laters did match what could be read on forums from
experience.
[Edited on 13-2-2009 by sylla]
stid - 3-9-2009 at 05:32
Sorry to pose my question so late.
So it is: is this possible to predict the chemical stability via computing way?
[Edited on 3-9-2009 by stid]
Polverone - 3-9-2009 at 09:45
Quote: Originally posted by stid ![](images/xpblue/lastpost.gif) |
Sorry to pose my question so late.
So it is: is this possible to predict the chemical stability via computing way?
|
It's considerably more involved, but I think the answer is yes. See for example this example which uses computational methods to explain the sensitivity of PETN's silicon analog.
stid - 3-9-2009 at 10:13
Thank you for the answer! And one question again: does some strict relation exist between the symmetry of the molecule and the chemical stability of
the substance?
Plasmapyrobattics - 3-9-2009 at 14:59
Quote: Originally posted by stid ![](images/xpblue/lastpost.gif) |
Thank you for the answer! And one question again: does some strict relation exist between the symmetry of the molecule and the chemical stability of
the substance? |
Not necessarily. It also depends on what you mean by “chemical stability”. Do you include sensitivity perhaps?
One finds various symmetrical energetic compounds exhibiting both sensitive, stable and (or) insensitive and/or unstable properties. Examples are :
1. 5,5-bis(nitrotetrazole) [very sensitive but relative stable].
2. 4,40-dinitro-3,30-azo-bis(furazan) [sensitive but relative stable].
3. octahydro-1,3,4,6-tetranitro-3aa,3bb,6ab,6ba-cyclobuta(1,2-d:3,4-d0)-diimidazole-2,5-dione [sensitive but relative stable].
4. 2,6-diamino-3,5-dinitropyrazine [relative insensitive and stable].
5. 3,30-azo-bis(6-amino-1,2,4,5-tetrazine) [relatively insensitive and stable].
6. cissyn-cis-2,6-dioxo-1,4,7,8-tetranitrodecahydro-1H,5H-diimidazo(4,5-b:40,50-e)pyrazine [relative insensitive and stable].
7. 1,3,4,-tetranitroglycouril [medium sensitivity and relatively (hydrolytically) unstable].
Hope this helps
stid - 12-10-2009 at 00:29
Hi,
I have calculated the density of HMX using the correction coefficient 0,955. The obtained density is 1,83 gr/cm3– very different from the
experimental value. But the no corrected value is very close – 1,91 gr/cm3. What happens? And what is the relation between the pm3 optimized
structure of HMX and his different real isometric structures?
Thanks
simply RED - 13-10-2009 at 07:37
PM3 is semiempirical method. The geometry optimized with it has nothing in common with the experimental one. Semiempirical methods give tremendous
errors when computing nitramines' properties with them. They are not parametrized for this kind of compounds.
Try ab-initio methods.
RHF with 6-31G gives good geometry and bond lengths similar to X-ray analysis.
DFT (B3LYP), MP2... Should give good results too.
stid - 14-10-2009 at 02:11
Thanks for your answer!
simply RED - 15-10-2009 at 07:23
One else thing to post : the energy, calculated with semiempirical method or RHF is WRONG. RHF excludes electron correlation and brings error to the
energy. It gives "nice" geometries somehow anyway...
It should be calculated at least with B3LYP or MP2, that you could believe in it. When calculating energy - use polarisation, diffusion and frequency
corrections. When calculating in crystal (multiple molecules), use ++ , **, freq and BSSE (basis set superposition error) ! At least with 6-31G !
By the way : if you want to calculate some properties of a chrystal, you should start with the X-ray analysis geometry (if you have it)! If you are
calculating properties of a new compound, you obviously have no X-ray to start with...
I know it needs extreme computational resources, but there is no other way !
[Edited on 15-10-2009 by simply RED]
stid - 20-12-2009 at 02:15
Quote: Originally posted by simply RED ![](images/xpblue/lastpost.gif) |
It should be calculated at least with B3LYP or MP2, that you could believe in it.
[Edited on 15-10-2009 by simply RED] |
Two months later,
Hi!
How can I command PCGAMESS to use B3LYP or MP2? Can I download from somewhere examples input files?
Thank you!
[Edited on 20-12-2009 by stid]
Engager - 20-12-2009 at 03:41
$CONTRL MAXIT=50 UNITS=ANGS COORD=CART RUNTYP=OPTIMIZE
SCFTYP=RHF DFTTYP=B3LYP $END
$GUESS GUESS=HUCKEL $END
$BASIS GBASIS=N31 NGAUSS=6 NPFUNC=1 NDFUNC=1 $END
$DATA
5-Nitro-1H-Tetrazole, optimization 63-1G** B3LYP functional.
C1
C 6.0 0.0101202824 -0.0433480092 -0.0646075395
N 7.0 0.8086734648 1.0941011978 -0.0948870086
N 7.0 2.0860823587 0.7103841160 -0.0935010466
N 7.0 2.1224873963 -0.5835695032 -0.0644757289
N 7.0 0.9068321991 -1.0745229357 -0.0464345781
N 7.0 -1.4875960040 -0.1257062031 -0.0542365103
O 8.0 -2.0397093943 -1.1913111230 -0.0261163789
O 8.0 -2.0665188892 0.9431247185 -0.0759871348
H 1.0 0.5390141506 2.0473502898 -0.1149126989
$END
stid - 20-12-2009 at 08:50
Thank you!
I will try.
The input coordinates of your example is the coordinates given of MM2 optimization of Chem3D?
[Edited on 20-12-2009 by stid]
Engager - 7-1-2010 at 04:58
Calculating brisance or shattering effect
Brisance is the destructive fragmentation effect of a charge on its immediate vicinity. When an explosive detonates,
tremendous pressure is released practically instantaneously in a shock wave which exists only a fraction of a second at any given place. The
subsequent expansion of gases performs work but the sudden pressure thus created will shatter rather than displace any object in its path. The ability
of an explosive to demolish (fragment, shatter) a solid object (such as steel, concrete, stone) when fired in direct contact with it or in its
vicinity is called brisance (from the French "briser" = to break or shatter). From a military viewpoint brisance is of practical importance because it
determines the effectiveness of an explosive in fragmenting shells, bomb casings, grenades, mines, etc and in imparting high velocities to the
resulting fragments. As the shattering effect is dependent upon the suddenness with which the gaseous products of an expl are liberated, the velocity
of detonation is at least a major factor in determining.brisance. It has been found that there is a general linear relationship between velocity of
detonation and brisance, and if the velocity is known it is possible to calculate the brisance or vice versa (as will be shown below under
Brisance-Detonation Velocity Relationship)Brisance may also be calculated from the formula of Kast (see below) or determined experimentally by one of
the test methods. Since brisance is approx proportional to detonation velocity, “force” and density of loading, Kast proposed to determine
it by the following equation:
B = F * d * D
Where В is brisance value (BrisanZwert in Ger), d is density of charge, D detonation velocity in m/sec and F
"specific energy or force", also called “specific pressure”. The Germans call it "spezifische Kraft oder Energie". The force is expressed
in kg/cm and is equal to p0 * v0 * T/273 where p0 is atmospheric pressure expressed as 1.033kg/cm2, v0 volume of gases developed on explosion in cc
per g of explosive, reduced to 0C and 760mm Hg pressure and T is the max absolute temperature of explosion. On substituting for F, in the above
expression, the following equation is obtained:
В = P0 * v0 * T/273 * d * D
In the above equation T is equal to t+273 or to Qe/C + 273 where Qe is the heat of explosion in cal/g and C is the
mean specific heat of the products of expln in cal/g. As an example, for blasting gelatin (NG 92 & NC 8%), Stettbacher gives: p0 = 1. 033, v0 =
711.4cc per g, T = 4410°C, d 1.60 and D = 7500 m/sec. This gives:
B= 1.033*711.4* (4410/273) * 1.6 * 7500 = 151.2E+6
Kast's values for many explosives can be found in references. However, practical tests do not confirm the idea that
В is proportional to the square of the deton velocity but that simple proportionality (as in the formula of Kast) agrees better with the facts.
Friederich introduced the term "specific brisance" and proposed to calculate it from the formula (D2max*A)/100 kg/cm2, where Dmax is detonation
velocity and A specific gravity in g/cc. The following table compares "specific brisance" with Kast's brisance values:
![](http://img697.imageshack.us/img697/8089/brisance1.jpg)
It should be noted that brisance is a very complicated phenomenon and that none of the existing methods of
calculation, such as by Kast's formula (see above), Herlin's formula, Bichel's formula, Friederich's formula, etc or of experimental determinations
gives exact interpretation of B. The matter of detg it is complicated by the fact that the В of a cartridge of explosive is different in
different directions: if a cylindrical cartridge is detonated from one end, the action in the direction in which detonation proceeds is considerably
greater than that in the opposite direction. According to Cook the term brisance was used to describe the property now attributed to detonation
pressure. This property may in many cases be calculated from fundamental physical laws. For a condensed explosive the detonation pressure p2 may be
approx calcd from the equation:
p2 = 0.00987*p*(D^2)/4
Where p, is the original density and D the detonation velocity in m/sec. A more accurate equation is also given by
Cook. Lothrop & Handrick discussing the relationship between performance and constitution of pure organic compounds included curves showing the
relationship between power & brisance and oxygen balance of many organic explosives. Price, in discussing the dependence of damage effects upon
detonation parameters of organic high explosives, substituted the term detanation pressure for brisance and detonation energy for power. She also
stated that from data obtained at NOL, it has been possible to show that fragment velocity, shaped charge penetration, airblast, and underwater
effects are related to the explosive properties of detonation pressure and detonation energy.
Brisance-Detonation Velocity Relationship.
Brisance-Detonation Velocity Relationship has long been recognized that brisance is related to detonation velocity
and efforts have been made to determine and express relationship beween these two characteristics of an explosive. According to Rinkenbach, there was
developed at Picatini Arsenal the following approx empirical relationship between brisance(B) in grams of sand crushed by 0.4g sample when detonated
in a 200-g bomb, and detonation ve-locity (D) in m/sec; logB= 3.451og(D/2450). A similar equation was later reported in a manual compiled at Aberdeen
PG. From sand test values (B) detd at PicArsn for ca 20 explosions (using 0.4g samples in both 200g and 1700g bombs) and from data available in the
literature for their deton velocities (D) at approx their max densities, Rinkenbach obtained a nearly linear relationship on plotting В vs D.
This permitted the following equations to be derived:
D = 63.99B + 4234 m/sec (for 200-g bomb)
D = 76.76B + 3965 m/sec (for 1700-g bomb)
By means of these equations the detonation velocity of an explosive can be calculated with a mean accuracy of ca 45
m/sec. Note: The above equations are not identical because the values for В obtained in the 1700-g bomb were somewhat lower than those obtained
for the same expls in the 200-g bomb; but the relative orders of the expls with respect to В were the same in both bombs. The difference between
the В values for each explosive in the two bombs is attributed to the different thicknesses of the layers of sand between the cap (contg the
chge) and the walls of the two bombs. Table below gives a comparison between D calcd by Rinkenbach and D obtained by averaging the various values in
the literature.
To calculate brisance of unknown compounds as discussed in this topic one can simply use above equations provided by
Rinkenbach:
B = (D – 4234) / 63.99 (200g bomb)
B = (D – 3965) / 76.76 (1700g bomb)
Using calculated VOD, for example in out test case we get (8899-3965)/76.76 = 64g of crushed sand, experimental
value for RDX at density slightly lower then TMD is 59g of crushed sand. As seen in this example, equations above can provide quite accurate
prediction of brisance.
Explosive Blasting Force
Power of Explosives. In its normally used context, power of an explosive is a misnomer. It is generally accepted
that power of an explosive is a measure of its strength, its blasting action or available energy, and not necessarily a measure of its rate of energy
delivery, which is indeed the true definition of power. Further confusion arises because another frequently used explosives term, called brisance, is
sometimes erroneously equated with power. Brisance is a measure of the ability of an explosive to shatter material in its immediate vicinity. The
fundamental property of an explosive that determines brisance is its detonation pressure. The power of an explosive (we bow to accepted usage and
will keep referring to power rather than the correct terms such as strength or blasting ability), on the other hand, is a measure of the ability of an
explosive to do work such as blasting down rock or propelling a chunk of metal. The fundamental explosive property that determines its power (or
better, available work) is its heat of detonation, Q, or the related quantity, njTj, where nj is the number of moles of gas under steady
(Chapman-Jouguet) detonation conditions and T; is the detonation temperature. As will be shown below, a more exact dependence is that power is
proportional to Q-q (rather than just Q), but q, the residual heat of the detonation products, is usually quite small compared to Q. According to
Andreev & Belyaev, taking to account that exposion process is substantialy adiabatic, the energy available to do external work (we continue to
miscall it power) is:
![](http://img690.imageshack.us/img690/4946/trauzl1.jpg)
Where P - pressure, V - volurne, T - ternperature, Cv - specific heat of the detonation products, and the
subscripts, i & f refer to initial and final states respectively. The initial state is usually taken to be that achieved in a constant volume
explosion, the final state is the state of product expansion, after which no more useful work is available. Final temperature of gasses is not easy to
predict, so to make equation more suitable for actuale use it’s more effective to use ratio of pressures instead of temperatures, so taking to
account equation of state for ideal gas we can derive equation above to the following form:
![](http://img121.imageshack.us/img121/6848/trauzl2.jpg)
Where K is adiabatic index (Cp/Cv), witch in common explosion conditions is aproximately 1.28 for diatomic gasses
and 1.17 for triatomic ones. Since gasses will expand until they equalize their pressure with surrounding ambience Pi is simply atmospheric pressure
~1 bar or precisely 101325 Pa. Pf – is initial pressure of expanding gasses, it can be derivated from calculated exposion temperature (watch my
posts about calculation of VOD by Keshwarz method above) and by taking to account the fact that at initial moment all explosion produced gasses occupy
space witch was occupied by initial solid exposive, so initial gas volume is Vi = m/r0, where m – mass of explosive, r0 – loading density.
Since equation of state will include ammount of gasses produced by explosion (Ng, moles of gas per mole of explosive), we should use volume of 1 mole
of explosive from witch this ammount of gasses is produced, so Vi = Mw/r0, where Mw is molecular mass of explosive. Substitution of this values into
equation of state for ideal gas (written for Ng moles of gas produced by explosion) gives us following equations:
![](http://img684.imageshack.us/img684/7243/trauzl3.jpg)
Here Pi – initial gas pressure (Pa), Pf – ambient pressure (101325 Pa), R – universal gas constant
(8.31), Ng – moles of explosion gasser per mole of explosive, Ti = Te = temperature of exposion (K), Mw – molecular mass of explosive in
(kg/mole), r0 – density of explosive (kg/m3), k – average adiabatic index of gaseous explosion products, Qe – heat of explosion
(MJ/kg), A – efferctive work of explosion (MJ/kg), Ne – explosion work efficency coefficent. Using equations above, with explosive density
(calculated as shown in previous posts), number of explosion gasses per mole of explosive (derivated from explosion reaction equation), explosion
temperature (also computed with calculation of VOD by Keshwarz method described in previous posts), we can now simply calculate effective work of
explosion for our model explosive, only additional parameter witch we need to calculate is K – average adiobatic exponent. Let’s look on
our model explosion equation again:
C3N6H6O6 = 3H2O + 3CO + 3N2
As we see 1 molecule of explosive produces 9 moles of gaseous products, from witch 6 moles are diatomic gases, and 3
moles are triatomic ones. Since K is simple average and for diatomic gasess for common explosion conditions k = 1.28 and k = 1.17 for triatomic ones
we calculate average K:
K = (6/9)*1.28 + (3/9)*1.17 = 1.243
For example let’s calculate effective explosion work for out model explosive from previous posts.For our model
explosive we calculated following parameters: T=3731K; r0 = 1.81 g/cm3 = 1810 kg/m3; Ng = 9; Mw = 222.11 g/mole = 0.2221 kg/mole; Pf = 101325 Pa ; Qe
= 5.668 MJ/kg (more accurately calculated using computed heat of formation for our model exlosive and experimental ones for explosion gasses); R =
8.31 ; K = 1.243, we get:
Ne = 1 - ((101325*0.2221) / (9*8.31*3741*1810)) ^ (0.243/1.243) = 1 - ((22504.2825) / (506418795.9))^(0.1954) = 1 – 0.1411 = 0.858 = 85.8%
A = Ne*Qe = 0.858*5.668 MJ/Kg = 4.868 MJ/kg
Values taken from literature are 86.6% and 4.710 MJ/kg respectively, so computed results are in nice agreement. For
example, below are corresponding values for some commonly used exposives, against their heats of explosion and corresponding ratios vs TNT and results
of Trauzl lead block expansion tests:
Now when we know exposive power we can compare it against corresponting value for some known explosive with known
power test value (for example lead block expansion - Trauzl test) and finaly derivate aproximate test value of explosive power test for our model
explosive. There are many explosive blasting power tests mentioned in literature, three of this methods are in common use: 1) Ballistic Mortar; 2)
Trauzl block expansion; 3) Underwater explosions; and 4) one method - cylinder expansion - that is now used at Lawrence Iivermore Laboratories.
Trauzl Test.
Trauzl Leod Black Test or Lead Black Expansion Test (Cavite au bloc de Trauzl or Epreuve au bloc de plomb de Trauzl,
in Fr) (Trauzlsche Probe or Bleiblockausbachung Methode, in Ger) (Prueba Trauzl or Prueba del bloque de plomo, in Span ) (Metodo del Trauzl or Metodo
del blocco di piombo, in Ital). This test measures the "comparstive disruptive power''of an explosive through enlargement of a cavity in a cylindrical
lead block under carefully standardized conditions. Standart conditions for conducting this test were defined by a Comm. of the Fifth International
Congress of Applied Chemistty. Although one of the oldest tests known for determinating power, it is still widely used today but more common in Europe
than in the USA Scheme of apparatus is shown below:
![](http://img695.imageshack.us/img695/2041/trauzl5.jpg)
Procedure. A sample of the test explosive (approximately 10 g) is detonated in a cavity or borehole, 25 mm in
diameter and 125 mm deep, in a standart lead block 200 mm in diameter and 200 mm in height. The borehole is made centrally in the upper face of each
block, previously cast in a mold from desilvered lead of the best quality. An electric blasting cap is placed centrally in the charge. After the
charge and detonator are placed in the borehole, 40 cm3 of Ottawa sand are added and tamped lightly. An additional 10 cm3 of sand are added and tamped
more thoroughly. The volume of the hole made due to the press exerted by the exploding charge is then detd; and the distension(expansion) is
calculated by subtracting from this value, the volume of the borehole before the charge is detonated. Three such tests are made and the results
averaged. Expansions for equivalent weights of explosives are calculated, and the test value is expressed in % of the expansion of an equivalent
weight of TNT. The Trauzl test in France is somewhat different in procedure although dimensions of the lead block are the same. Initiating efficiency
strength of primary explosives can be approximately determinated by firing a small charge (such as 1.0 g) in the cavity of a small lead block, such as
100 mm in height and 100 mm in diam. For testing detonators in such block, a hole is bored in the block of the exact diam of the detonator and of such
a depth that the top of the detonator is flush with the top of the block.
Calculating Trauzl Test Value
As clearly seen from test description above trauzl test results are clearly product of explosive blasting power,
determined by effective work of exposion. To derivate trauzl test results for our model explosive we must compare effective work of explosion of our
explosive against effective work of explosion for some other known explosive with measured Trauzl test. To do so we must enstablish effective work of
explosion equavalency and after that use a graph of Trauzl value vs weight of charge for this known explosive to determine value of Trauzl expansion
for our model explosive. A suitable explosive for comparsion is Ammonite №6, proposed by Andreev & Belyaev due to almost complete
independence of explosion energy from density. Andreev & Belyaev in their book on explosive theory provide the following graph:
![](http://img253.imageshack.us/img253/1420/trauzl6.jpg)
Let’s estimate Trauzl Block test value for our modell explosive, to do so the only thing we need is value of
effective work of explosion, witch we calculated in section earlier, for our model explosive (RDX) we calculated Ae = 4.868 MJ/kg ; using data from Ae
table in corresponding section we find Ae for ammonite №6 Ae = 1030 ccal/kg = 4.312 MJ/kg. After subdivision of corresponding values we can
calculate our explosive/ammonite6 eq. ratio and calculate corresponding Trauzl test estimate value for our explosive:
Ae/Ae(ammonite) = 4.868 / 4.312 = 1.128; Eq.w.(ammonite6) = 10*1.128 = 11.28g
Using graph above we get Trauzl test value for our explosive, aproximately 480 cm3, experimental value for RDX is
495 cm3, so method is usefull and can provide results with good align with experiment.
In addtion to this descriptions i have modified detonation calculator utility, now it also calculates effective work of explosion and computes
brisance and blasting power values.
Also i've added blast wave calculator module witch use Sadovsky formula to calculate excessive pressure in front of blast wave at requested range from
explosive charge, using heat of explosion and explosive mass. In addition it creates a report, showing effects of this explosive charge vs uncovered
human and buildings on different distances, calculating hazard radiuses for several types of dammage effects. Theory of blast wave computation will be
posted in this thread some time later when i will have more free time.
[Edited on 7-1-2010 by Engager]
Attachment: Detonation Utility.rar (46kB)
This file has been downloaded 1016 times
franklyn - 8-1-2010 at 02:59
Very good work Engager , physical performance of explosive materials is a
topic which yet remains to be adequately expressed from calculation alone.
Characteristics that will yield good performance are understood, but are not
easily estimated computationally.
Your utility applying such methods gives essentially the same results for the
hypothetical compound I proposed here , corroborating that the estimate is
correct.
http://www.sciencemadness.org/talk/viewthread.php?tid=11195&...
Attached below the output of your latest Detonation Utility.
Detonation Utility by Engager
Keshavarz = 9059 , Eisenstadt = 8631
Velocity of Detonation calculated by :
M.J. Kamlett,
S.J. Jacobs = 9208 - 6% correction = 8656
HE calc by enhzflep = 9370
http://www.sciencemadness.org/talk/files.php?pid=64852&a...
___________________________________
@ Engager
Your utility is easy to implement if one understands what the labels ask
but there are subtle issues that I only now discovered which are not
apparent and kept me from applying the earlier version before.
When the utility is initialized the space for " Target density (g/cm3) "
contains an entry which has a coma after the first digit ( 1, ). If one
replaces the 3 digits to the right after this coma ( ,816 ) and runs the
program , a window (attached below) asserting
" Target density must have realistic value " is displayed.
The program will not run for any value greater than ( 1 ).
For the program to work at all for density values greater than ( 1 )
the coma of the initial entry must be deleted and replaced with a period.
.
![Info.JPG - 7kB Info.JPG - 7kB](http://www.sciencemadness.org/talk/files.php?pid=169143&aid=9384)
Engager - 8-1-2010 at 09:59
Quote: Originally posted by stid ![](images/xpblue/lastpost.gif) |
Thank you!
I will try. The input coordinates of your example is the coordinates given of MM2 optimization of Chem3D?
|
I don't remember where i taken them, but it's probable that i used common way Chem3D => Gamess RHF, mini basis for initial low cost optimization
=> coords for heavier 6-31G basis set. Sometimes i want even more precise results and use wide basis with extremely computational costly MSCSF
(Multi-configurational self-consistent field), starting on orbitals provided by 6-31G.
Quote: Originally posted by franklyn ![](images/xpblue/lastpost.gif) |
Your utility is easy to implement if one understands what the labels ask
but there are subtle issues that I only now discovered which are not apparent and kept me from applying the earlier version before.
When the utility is initialized the space for " Target density (g/cm3) " contains an entry which has a coma after the first digit ( 1, ). If one
replaces the 3 digits to the right after this coma ( ,816 ) and runs the program , a window (attached below) asserting " Target density must have
realistic value " is displayed. The program will not run for any value greater than ( 1 ).
For the program to work at all for density values greater than ( 1 ) the coma of the initial entry must be deleted and replaced with a period.
|
Thanks, now i finally understand the nature of this problem - it's in locale metrics setting in windows. Here in Russia we use "," to separate number
from fractional part, but in US locale "." is used to do the same. If i run program on my machine and try enter "1.87" it results in error, because
programming language (Visual Basic 6) misinterpreted such input due to my Russian locale setting in windows in witch "," is separator for fractional
part - for VB in my locale value "1.87" is not interpreted as numeric !!!. That's why density "1,87" is shown on initialization. However i don't quite
sure with locales use "," and witch use ".", how can i place correct initialization value then i don't know locale at witch my utility will run?
Franklyn, how do you suggest?
Engager - 8-1-2010 at 10:38
Quote: Originally posted by simply RED ![](images/xpblue/lastpost.gif) |
One else thing to post : the energy, calculated with semiempirical method or RHF is WRONG. RHF excludes electron correlation and brings error to the
energy. It gives "nice" geometries somehow anyway...
It should be calculated at least with B3LYP or MP2, that you could believe in it. When calculating energy - use polarisation, diffusion and frequency
corrections. When calculating in crystal (multiple molecules), use ++ , **, freq and BSSE (basis set superposition error) ! At least with 6-31G !
By the way : if you want to calculate some properties of a chrystal, you should start with the X-ray analysis geometry (if you have it)! If you are
calculating properties of a new compound, you obviously have no X-ray to start with...
I know it needs extreme computational resources, but there is no other way !
[Edited on 15-10-2009 by simply RED] |
You are absolutely right, but using costly methods exactly at start it's madness, you will wait for long time (many hours or even days in cases with
big number of atoms or if initial structure guess is bad), especially on heavy basis set... Using PM3 for initial optimization is a generally good
idea, since it fast and WILL converge in most cases. If one needs more precision i recommend to get converged PM3 structure and then => 6-31G + RHF
to get orbitals => MCSCF + MCQDPT. However this will require too much computer time to get this nasty stuff to convege, for general unexperienced
user it is madness, what's why i shown the simplest way first. Advance can always follow.
[Edited on 8-1-2010 by Engager]
franklyn - 8-1-2010 at 12:24
@ Engager
Programming is something I have only a passing acquaintance with.
I would just use variables to equate coma ( , ) and period ( . ).
coma , ( , ) = Varible ( . ) , period
period , ( . ) = Variable ( , ) , coma
or else
use " go to " command
if ( , ) go to ( action )
if ( . ) go to ( action )
.
thanks again
Formatik - 8-1-2010 at 14:58
The program works excellent.
[Edited on 9-1-2010 by Formatik]
Engager - 8-1-2010 at 18:58
Long way to the truth....
Finally i've found source of issues with input in earlier versions of utility. It took quite a bit of effort to understand problems with utility witch
various people have encountered. There was a big problem in microsoft software - more precisely in locale issues, problem was that different locales
use different symbols as separator for full and fractional parts of number. In Russia "," is used to separate full part of number from fractional so
if i ran program on my computer everything was just fine since i followed my locale numbering rules, but everyone from US has problems because
software conversion of "," raises a error due to different separator used in their locale ".". At first i though that that is the only problem but it
is not, and only then i switched my locale to US one i found that system interpret entered value "1,234" not as error but as 1234 since "," is used in
US locale to separate thousands, million and so on. Only after this i finally recognized in what exactly is the problem and was able to fix it. Thanks
to franklyn and Formatik for their help in support resolving this issue! I have to apologize for everyone who downloaded my utility and suffered from
input problems, even if this is not exactly my fault, but is fault of unpredicted behavior of programming language in US locale. Repaired version of
utility & source code on VB6 is attached to this message.
I convincingly ask any moderator who read this message to remove attached previous versions of my utility earlier in this
thread since i can't edit my message anymore and leave only last one attached to this message, so nobody else suffer confusion from this input locale
problems!
Attachment: Detonation Calculator Utility (Input issue bugs fixed).rar (47kB)
This file has been downloaded 1661 times
[Edited on 9-1-2010 by Engager]
franklyn - 11-1-2010 at 11:26
@ Engager
Your detonation calculating algorithm is outstanding ,
your coding solving the country convention of
numeric entry is even more remarkable.
Now it's universal !
.
Engager - 2-1-2011 at 18:39
In some post earlier in this topic i've promised to write about calculation of blast wave parameters and about action of blast wave against people and
buildings, it is now posted in this topic:
http://www.sciencemadness.org/talk/viewthread.php?tid=15150#pid=197153
I add this link here for convenience of people who wish to expand information from this topic with some details of blast wave calculation for any
actual explosion case.
simply RED - 5-1-2011 at 01:52
About the quantum calculations.
PM3 and AM1 give good starting geometries whan calculating organic molecules (saturated, unsaturated, amines, alcohols, carb. acids etc). Anyway,
those methods give tremendously wrong geometries when calculating nitramines. They underestimate the N-NO2 n-pi conjugation and instead of planar or
close to planar (depending on other interferences) geometry of the system (as all X-ray data and high level calculations show) they give trigonal
pyramide like ammonia.
And yes, the starting geometry should be the closest possible to the one that the method will give as a result, or you have to wait loooong time the
geom opt to converge.
I recommend direct HF or B3LYP geometry optimization (from X-ray data or AM1, PM3 start) with 6-31G (DZVP) basis set. And then recalculate (again geom
opt, not just single point) with at least with 6-311+G* (TZVP). If you have computational resources I recommend direct MP2 or better (faster) RI-MP2
geometry optimization all in the RAM. Direct MP2 geom opt with 4 processors sometimes tend to converge faster than even B3LYP on 8 processors, because
the DFT opt modules (both GGA and Hybrid) sometimes has the bad tendency to oscillate the energy at the end of the optimization - especially with the
Gaussian program. MP2 gives 90% of the correlation energy when calculating ground states of the molecules, this gives you 95+% correct results for
energies or geometries! MP2 is not the best for excited states or transition states, MP4, CCSD or MCSCF(SD) work for these cases. Some say TDDFT works
also, but I've never tried...
For the enthalpy of detonation calculations you need BSSE, ZPE and temperature corrections (vibrational, rotational and translational temp corrections
to the energy) in order to get good results.
Serious calculations can not be done on single processor. Anyway, modern multicore PC processors with very good cooling and AT LEAST 16GB RAM provide
good perspectives for the amateour quantum chemist.
It would be good if the forum has its own "super" computer with lets say 8 or 16 cores and 32 GB RAM. Then we could log in there and do energetic
materials calculations. Because even if you have access to academic supercomputer you can not do energetic materials calculations there or you will be
expelled from the institution.
Mods? Spare money from donations?
[Edited on 5-1-2011 by simply RED]
DubaiAmateurRocketry - 25-1-2014 at 10:27
Does any one know what shall I do when I see this ?
I downloaded the file and when i tried to open the calculator this appears. I know almost nothing in this field.
![](http://i41.tinypic.com/fmrr84.jpg)
Dornier 335A - 26-1-2014 at 03:36
His calculator doesn't seem to work on Windows 7. It does work on Windows XP however.
VladimirLem - 26-1-2014 at 07:06
I have the same problem
(Windows 7 here)
Does anyone know how to fix that?
Dornier 335A - 26-1-2014 at 07:54
I have tried to run it in compatibility mode in every way. The problem must be that he compiled it on Windows XP and it requires that DLL to work
correctly.
VladimirLem - 26-1-2014 at 08:36
well...can anyone upload that file?
franklyn - 26-1-2014 at 14:11
Download the msstdfmt.dll. here => www.dllrepair.com/dll/dll-files/msstdfmt.dll
or here => www.dlldump.com/dllfiles/M/MSSTDFMT.DLL
When the window prompting the destination appears , copy and paste this in
If you have a 32 bit version of Windows 7, send the file to => C:\WINDOWS\system32 ,
this puts it into the System32 folder of Windows
or
for the 64 bit version of of Windows 7, send the file to => C:\WINDOWS\SysWOW64 ,
this puts it into the SysWOW64 folder of Windows
Now you need to register the file into the operating system's registry hive as follows.
Click Start at the lower left on your desktop for the Start menu.
Go to Accessories and locate the Command Prompt.
Right click on the icon for the Command Prompt and select Run as Administrator.
When you see the black console window , copy and paste the following command ,
for 32 bit Windows 7 users => C:\WINDOWS\system32\regsvr32.exe Msstdfmt.dll
and for 64 bit Windows 7 users => C:\WINDOWS\SysWOW64\regsvr32.exe Msstdfmt.dll
then hit the enter key on your keyboard
Done
.
DubaiAmateurRocketry - 27-1-2014 at 04:49
Thanks for the guide franklyn!!! however .... Ops... and I still can not open the detonation calculator.
![](http://i42.tinypic.com/t54129.jpg)
[Edited on 27-1-2014 by DubaiAmateurRocketry]
franklyn - 27-1-2014 at 10:40
You definitely have registry errors
So do as it says , Google " error 0x8002801c "
Some selections
• The file is different but the solution is the same
www.bharathtech.com/2010/04/registering-ocx-control-in-windo...
www.youtube.com/watch?v=jWiBkU9soRU
• www.cryer.co.uk/brian/windows/troubleshooting/nt4_dllregiste...
• Try running some of the registry fixer programs offered.
Windows RepairAll In One _
www.bleepingcomputer.com/download/windows-repair-all-in-one-...
Glary Registry Repair _
www.snapfiles.com/downloads/gregrepair/dlgregrepair.html
Reimage Repair _
www.reimageplus.com/lp/sys/index.php
.
VladimirLem - 27-1-2014 at 11:46
C:\WINDOWS\system32\regsvr32.exe Msstdfmt.dll
C:\WINDOWS\SysWOW64\regsvr32.exe Msstdfmt.dll