[*] posted on 9-11-2013 at 13:34
Electrolyzing NaOH: finally succeeded !


Finally I electrolyzed NaOH. The first time with success. In a large stainless steel soup dipper I melted NaOH prills (which got brown due to dissolved metal oxides from the stainless steel and the copper cathode).
I used a copper strip as cathode and the dipper itself as anode. I used an 8 Amp battery charger and a halogen bulb in series to prevent short circuiting. There were some small explosions due to water vapor from the anode reacting with the Na metal. I had to keep the temperature near freezing, i.e. between 320 and 330 C to prevent dissolving of the Na metal in the lye. It was not easy to pick the small (liquid) Na balls (3-5mm) from the bath, they slipped easily back into the bath, but I got some in the lamp oil.


<iframe sandbox width="640" height="360" src="//www.youtube.com/embed/Lp1SC9UWyRo" frameborder="0" allowfullscreen></iframe>

[Edited on 2013-11-9 by metalresearcher]
View user's profile View All Posts By User
Random
International Hazard
*****




Posts: 1018
Registered: 7-5-2010
Location: In ur closet
Member Is Offline

Mood: Energetic

[*] posted on 9-11-2013 at 13:54


Good work, I hope you can improve the procedure with a bigger yield in the future. Molten NaOH looks scary though, I bet it would eat away all flesh to the bone at that temp.
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 9-11-2013 at 14:01


A side question please, when sodium forms at the cathode, why does it not simply react with hydroxide to form sodium oxide and hydrogen gas by this reaction:

2Na + 2NaOH => 2Na2O + H2

What I'm trying to get at is why use NaOH melt if it is still a protic 'solvent'/electrolyte of sorts no?

[Edited on 9-11-2013 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 9-11-2013 at 14:28


Quote: Originally posted by deltaH  
A side question please, when sodium forms at the cathode, why does it not simply react with hydroxide to form sodium oxide and hydrogen gas by this reaction:

2Na + 2NaOH => 2Na2O + H2



I think you'll find the answer to ALL your questions on NaOH(l) electrolysis here:

http://www.sciencemadness.org/talk/viewthread.php?tid=9797

In short, this is how it's done! len1 must be one of the very few in the entire world to have built a lab scale functioning Castner cell. Hats off, once again. :):):)




View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 9-11-2013 at 14:31


Thanks for the link blogfast and hats off from me too... very brave experimentalist! I would have been petrified!



Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 9-11-2013 at 14:34


Quote: Originally posted by deltaH  
Thanks for the link blogfast and hats off from me too... very brave experimentalist! I would have been petrified!


He was probably the best experimentalist here on SM in recent years. Sadly he doesn't stop by too often anymore.




View user's profile View All Posts By User
WGTR
National Hazard
****




Posts: 971
Registered: 29-9-2013
Location: Online
Member Is Offline

Mood: Outline

[*] posted on 9-11-2013 at 23:21


metalresearcher congratulations on joining the sodium club! We look forward to hearing more of your exploits in the future.
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 732
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 10-11-2013 at 02:32


Well, I have tried another run, I was able to collect sodium again but there are a few issues. It is a thick brown slurry which makes collection difficult.
The reason is probably that I use the stainless steel container itself as an anode and the brown and yellow slurry is dissolving Cr2O3 and Fe2O3 from the attacked stainless steel.
And I don't want to heat it too much otherwise the Na metal dissolves into the lye.
So my next setup will be a separate anode (nickel).
In the collected items (second photo) there is a lot of frozen NaOH + metal oxide crud.

IMG_8727.JPG - 75kBIMG_8728.JPG - 64kB
View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 10-11-2013 at 05:57


Metalresearcher: this kind of set up is definitely a valid way of preparing small amounts of sodium metal in the lab. A.F. Holleman describes it in 'Inorganic Chemistry'. But you need nickel to take this any further. The sodium metal is usually collected using a metal gauze spoon.



View user's profile View All Posts By User
Fantasma4500
International Hazard
*****




Posts: 1681
Registered: 12-12-2012
Location: Dysrope (aka europe)
Member Is Offline

Mood: dangerously practical

[*] posted on 10-11-2013 at 06:41


i think the metal alloy might be problematic for this.. 316 works decently for handling NaOH, although food grade steel is not always that good for electrolysis for some reason
there is another alloy thats relatively common thats better for caustic enviroments however.. i suppose this would be better for molten NaOH
not sure if the more resistant steel was 308L?




~25 drops = 1mL @dH2O viscocity - STP
Truth is ever growing - but without context theres barely any such.

https://en.wikipedia.org/wiki/Solubility_table
http://www.trimen.pl/witek/calculators/stezenia.html
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 732
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 15-11-2013 at 13:00


What about using candle wax (paraffin) on top of the lye ?
The paraffin boils @ 370C (according to the largest online chemistry textbook) so above the electrolysis temperature (320-330 C) and protects the Na metal against air ?
Or is this a very bad / unsafe idea as the candle wax ignites easily @ 330 C ?

View user's profile View All Posts By User
bbartlog
International Hazard
*****




Posts: 1139
Registered: 27-8-2009
Location: Unmoored in time
Member Is Offline

Mood: No Mood

[*] posted on 15-11-2013 at 13:27


Cast iron is a better choice than most regular steel alloys. A nickel plated vessel would be even better, though. As for trying to cover the lye with some nonreactive fluid, I can't think of anything that would work. Easier to just have a lid once you get to the point where you don't need to observe the reaction the entire time.



The less you bet, the more you lose when you win.
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 15-11-2013 at 14:58


metalresearcher, a silver plated spoon or one marked EPNS might make a good anode. Silver oxide decomposes at 280C, so in molten sodium hydroxide temperature, it shouldn't even form, plus EPNS stands for electroplated nickel silver, so the nickel is there as well! Just make sure there's a decent layer of the plating left on your spoon, if there are deep scratches or worn off patches, it will probably corrode from there quickly! However, I wouldn't use one that has any value!

Using wax for your system is not a good idea. This is because long aliphatic hydrocarbons have very low autoignition temperatures, for example why diesel is used in diesel engines. Polyaromatic hydrocarbons (PAHs) have much higher autoignition temperatures (usually much higher than their bp), but their flash points are still roughly half of their boiling points! So one sparc and it WILL ignite :o NOT safe either, plus they are carcinogenic!!!

Polyethylene might work as a shielding melt, but you would need to research the safety of this FIRST!

[Edited on 16-11-2013 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 16-11-2013 at 06:09


Greatly increasing the chances of a fire involving molten lye isn't clever, IMO.

How about trying an imperfect Ar blanket by gently blowing welding argon over the melt's surface?




View user's profile View All Posts By User
m1tanker78
National Hazard
****




Posts: 685
Registered: 5-1-2011
Member Is Offline

Mood: No Mood

[*] posted on 17-11-2013 at 13:14


Quote: Originally posted by metalresearcher  
[...]
In the collected items (second photo) there is a lot of frozen NaOH + metal oxide crud.


Keep this cruddy sodium. A while back I posted a set of procedures to recover pure sodium from NaCl-sodium crud. Should work for NaOH-sodium crud too. It helps to smash the bits first.

As for the melt, remember that oxides and carbonates (to name a couple) poison your NaOH melt by raising the temperature needed to keep it molten. You'll instinctively raise the heat and/or current and wonder why much of the sodium is diffusing back into the melt.

If you have argon available (as blogfast suggested), try building a hedge around your crucible and gently blow in some Ar. This should extend the useful life of your electrolyte some.

Tank