Extraction of beryllium from beryl
So I just bought 3 pound of beryl ore, which is not cheap, soon it should be in my mail. Fallowing yield stated by Ullmann's I should get 44-45g of
beryllium. When I will get it I will make some test and post the results!
I never asked for this.
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
I just go the 3 pounds of beryl ore, in a few hour you should get my first thought and test about it. The beryl is crude, as expected, but do not
contain much gange. It is a pale blue/green/gray ore in 3/4 pieces.
I never asked for this.
|
|
Hexavalent
International Hazard
   
Posts: 1564
Registered: 29-12-2011
Location: Wales, UK
Member Is Offline
Mood: Pericyclic
|
|
Nice plante, I know you will, but please do be very careful with beryllium and its compounds!
"Success is going from failure to failure without loss of enthusiasm." Winston Churchill
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
Well, this rock is the most hard I ever saw! At first I took two piece of total 21.5 g total weight. At first I put the two pieces in 3 plastic bag
and smashed with a 16 ounces hammer, the hammer resonated in my hand, but the ore was untouched. Then I took the vise and put a bag under it. Then I
put the two pieces in the jaw and crushed them, it took 5 run before a good part of the ore was crushed to frit. 14 g of frit was obtained and 6.6 g
pieces. About 0.9 g was lost during crushing. The frit was mixed with equivalent weight of calcium carbonate. It was heated in a S.S 40ml crucible and
heated orange red hot and poured while hot in 50ml of cold water. Then 15ml Conc. H2SO4 was added and a lot of effervescence was observed as well as
strong sulphuric acid odor and hydrogen sulphide smell.
5 g (NH4)2SO4 was added to a beaker, and the sulphuric acid/beryl mixture was filtered in the ammonium sulphate.
While the mixture filtered and ammonium sulphate dissolved in the filtrate, a 13g piece of beryl was heated to yellow temperature and dropped in 50 ml
of cold water. The rock did not flinch so I re heated the ore to yellow temp, and dropped it in 200 ml cold water. The ore didn't seam to bother
thermal shock at all. While I heated the ore, I was expecting the ore to explode by air or steam. But it didn't happen. I'm starting to think that
berylware would make an awesome glassware!
I looked at the filtrate from the calcium carbonate reaction, and found small crystals starting to form at 20 degree Celsius. I put the beaker in the
snow outside, At the moment I wait for the mixture to precipitate most of the ammonium alum.
I had a face shield, and no dust was present during all the experiment.
[Edited on 10-1-2013 by plante1999]
I never asked for this.
|
|
barley81
Hazard to Others
 
Posts: 481
Registered: 9-5-2011
Member Is Offline
Mood: No Mood
|
|
Beryl is hard stuff. Mohs hardness 7.5! I'm glad you could crush some of it for experiments. I hope the rest of the procedure goes well for you.
Happy new year!
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
Yea, I just experienced its hardness! I just tried to powder 2 gram of frit I made using two steel plate and using pressure and movement to crunch to
powder. All I did was making heavy marks on the steel... This experiment will be challenging for me, at least I have 3 pounds of ore to test with! So
the precipitate, when at -2, by look was less than I tenth of gram.... For 14g worth of ore. The solution was discarded because of it's very low
concentration.
I need more aggressive chemical to dissolve the ore, saddly enough I do not have anymore NaOH left... I will try to find something else.
"I need something stronger"
Happy new year to you, and for every other member!
[Edited on 10-1-2013 by plante1999]
I never asked for this.
|
|
woelen
Super Administrator
       
Posts: 8082
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
I expect molten KF/KHF2 will do the job, but this is really nasty stuff. Not something to try at home in my opinion.
Btw, your results, although not very encouraging at the moment, are interesting. They demonstrate that BeO indeed is a dificult material to treat
mechanically and chemically. I have finely powdered pure BeO and this has proven to be extremely inert, but as I wrote before, I only tried dissolving
in all kinds of hot aqueous concentrated solutions. I did not try any melts.
[Edited on 10-1-13 by woelen]
|
|
12AX7
Post Harlot
   
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
Apparently beryl expands very little indeed, ~2.7 ppm/C, on par with borosilicate. It's probably even lower, amorphous. Berylsilicate glassware
indeed 
Tim
|
|
ScienceSquirrel
International Hazard
   
Posts: 1863
Registered: 18-6-2008
Location: Brittany
Member Is Offline
Mood: Dogs are pets but cats are little furry humans with four feet and self determination!
|
|
I think that you are not hitting it hard enough, fluoride containing fusion mixtures look like the way to go;
http://en.wikipedia.org/wiki/Berylium#Production
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
I would like a part of the thread to be put in chemistry in general and named extraction of beryllium from beryl. (For the moderators) Thanks!
Tonight I will try to react molten sodium pyrosulphate (made with sodium bisulphate) with the beryl frit. The objective is to solubilise the aluminium
and beryllium but not the silica. Then neutralize and leach with sodium bicarbonate solution for the beryllium content. The leach will then be boiled
to precipitate the beryllium hydroxide. Calcination and washing should give good purity.
I may also heat a beryl piece to yellow temp and drop cold water onto it while it is heated.
I do not have anymore fluoride, like I already said, it is one of the chemical I use the most. So now I must do without it. 1kg of calcium fluoride
would probably be well enough for the 3 pounds of beryl.
I want berylsilicate ware!
--------------------------------------------------------------------
EDIT (woelen): Thread is split and part on beryl ore is moved as requested.
[Edited on 10-1-13 by woelen]
I never asked for this.
|
|
woelen
|
Thread Moved 10-1-2013 at 06:07 |
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
Quote: Originally posted by woelen  | I expect molten KF/KHF2 will do the job, but this is really nasty stuff. Not something to try at home in my opinion.
Btw, your results, although not very encouraging at the moment, are interesting. They demonstrate that BeO indeed is a dificult material to treat
mechanically and chemically. I have finely powdered pure BeO and this has proven to be extremely inert, but as I wrote before, I only tried dissolving
in all kinds of hot aqueous concentrated solutions. I did not try any melts.
|
Fluorides, especially complex fluoride such as Na2FeF5 and Na2SiF6 are supposed to eat trough it like a charm. However I am out of stock for
fluorides. Some other agresive reagents at high temperature may be efficient too. Beryllium hydroxide leach in sodium bicarbonae solution. And
reprecipitate when the bicarbonate is decomposed by heating.
Thank you for splitting the thread.
I never asked for this.
|
|
Wizzard
Hazard to Others
 
Posts: 337
Registered: 22-3-2010
Member Is Offline
Mood: No Mood
|
|
I have a broken Argon laser which has an ID'd beryllium ceramic lasing vessel.... Dare I disassemble it?
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Years ago I found some interesting patents relating to extracting beryllium from Beryl, mostly by fusion with CaCO3. Not for the faint of heart!
This webpage here:
http://www.surechem.org/index.php?Action=document&docId=...
... is fairly wide in it's listing of beryl extraction technologies.
[Edited on 10-1-2013 by blogfast25]
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
I got my first beryllium hydroxide! I obtained a negligible amount, but still. I used my last 8 g of sodium hydroxide tough. First I took 2 g of
beryllium frit and mixed with 8g of sodium hydroxide in a S.S crucible and melted to a glass-like material. Then I dropped 30 ml of cold water onto
the glass. I poured the mixture to a beaker and added 20 ml of sulphuric acid, I wanted to use 10 ml but I used the wrong beaker. Then I filtered and
added 2 g (NH4)2SO4 and the solution was left in the cold for one day. The second day some crystalline material was precipitated. During the day I
found about bicarbonate leaching of beryllium, so I tried it. I added in 3 portion 300 ml of 10% NaHCO3. In the first 100 ml, effervescence was made.
in the second part some gelatinous precipitate formed, and the last 100ml made the mixture more fluid. The mixture was filtered and boiled to
precipitate the beryllium. I got a pinch of white flocculant precipitate, which I assume is beryllium hydroxide. The precipitate may be only a few
tenth of mg.
I also tried to grind thermally shocked beryl. It was found to be much easier. This is similar to the statement made in De Re Metallica, he say that
when the ore is heated and dropped in water, it greatly help to crunch it to a powder.
I never asked for this.
|
|
gregxy
Hazard to Others
 
Posts: 421
Registered: 26-5-2006
Member Is Offline
Mood: No Mood
|
|
There are also some Cu - Be alloys that might make
good starting materials. (probably fairly expensive though).
http://en.wikipedia.org/wiki/Beryllium_copper
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
So, here my actual plan for the week-end, which start today after school:
Because I found that thermally chocked ore are way easier to grind, I will do this treatment to 60 g ore and grind it. The basic melt seams to be
viable, so I will take 55 g of ore powder, and mix it with stochiometrical weight of sodium carbonate. I will heat to melt everything together, and
grind it to powder. I will add the powder to 200 ml water and I will boil it to try to dissolve the melt powder. Then I will add 92 ml of H2SO4 and
boil the mixture for a few tenth of minutes, to dissolve most of the aluminium and beryllium. I will filter to remove silica and sodium sulphate.
At this point I can do 4 treatment to extract the Be out of the solution. Which one should I use?
1: Precipitate the aluminium as Ammonium alum, filter and boil to get 90% + pure beryllium sulphate.
2: Add a few hundred ml of sodium bicarbonate solution, filter and boil to get 99% beryllium hydroxide/sub carbonate.
3: Add ammonia, filter, wash put it in ammonium chloride solution, and boil it to dissolve the basic beryllium hydroxide to beryllium chloride. Filter
and boil down to get 95% + Berryllium chloride
All these are from patents/ Ulmann's.
[Edited on 11-1-2013 by plante1999]
I never asked for this.
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Nice work indeed, plante!
Eliminating most of the aluminium as ammonium alum may be a partial solution to the problem: acc. Wiki, at 0 C, 100 parts of water dissolve only 2.62
parts of ammonium alum. My own observations confirm that more or less: I’ve made ammonium alum many times, also in kg quantities, and get near 100 %
actual yield, when chilling the solution to near 0 C.
Of course your supernatant liquor, assuming it still contains all the BeSO4 and there is no co-crystallisation, will still contain
some aluminium. Perhaps as final purification, exploit the differing degrees of amphoterism of Al and Be? Using a mild alkali like
bicarbonate it may be possible to keep the small amount of remaining Al in solution as aluminate, while 100 % precipitating the Be(OH)2?
Also, could you point to a few of the more interesting patents you’re using?
(It's really this bit I'm interested in:
Quote: Originally posted by plante1999  | During the day I found about bicarbonate leaching of beryllium, so I tried it. I added in 3 portion 300 ml of 10% NaHCO3. In the first 100 ml,
effervescence was made. in the second part some gelatinous precipitate formed, and the last 100ml made the mixture more fluid. The mixture was
filtered and boiled to precipitate the beryllium. . | )
Check your U2U.
[Edited on 11-1-2013 by blogfast25]
|
|
IrC
International Hazard
   
Posts: 2710
Registered: 7-3-2005
Location: Eureka
Member Is Offline
Mood: Discovering
|
|
Quote: Originally posted by Wizzard  | I have a broken Argon laser which has an ID'd beryllium ceramic lasing vessel.... Dare I disassemble it? |
Wear a dust mask, and avoid creating small particles. In short do not go cutting or grinding away on it. Also best to wear gloves to prevent any tiny
particles from getting into any broken areas on your skin (cuts). I like the bag of 50 for 4 bucks Vinyl gloves at Dollar store for stuff like this.
So thin you have full feeling and dexterity in your fingers. Not much protection for that reason but just avoid fracturing, cutting, or in general any
process which will create dust. In its unbroken, clean, solid form BeO ceramic is not too much to worry about. You can handle clean smooth Be metal
without any danger for the most part (within reason, being careful), but I still use gloves for the metal as well. The solid ceramic like the solid
metal is reasonably safe. It is when microscopic particles get into cuts or inhaled problems arise. No one desires to turn blue and die AFAIK. When
you need to transfer much heat while insulating against high voltages BeO in plate form is amazing stuff and safe when one is careful.However if you
do develop a sensitivity to either material it is time to stop playing with it.
"Science is the belief in the ignorance of the experts" Richard Feynman
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
If my calculations are correct, at 0 C a saturated solution of ammonium alum in water would contain less than 0.1 % of aluminium (as Al), based on
relative mass of alum at 453.33 g/mol and Wiki's stated solubility.
I may run a quick test with that...
[Edited on 12-1-2013 by blogfast25]
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
So I got a yield, finally!
First I mixed 10.6 g of anhydrous sodium carbonate and 5.5 g of beryl frit. I melted the two together until formation of CO2 stopped, it took about 30
minutes at yellow heat. Then the cooled material was put in 100 ml of cold water and boiled to dissolve a part of it. Then 40 ml of 30% HCl was added
and boilled until only a few grams of precipitate on the bottom. It was filtered and boiled down to give very crude beryllium chloride. Theoretical
purity is 15% beryllium chloride, the yield was 5g.
In industry they use alum precipitation.
For the bicarbonate patent: http://www.google.ca/patents/US2298800?pg=PA4&dq=berylli...
I never asked for this.
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by plante1999  | First I mixed 10.6 g of anhydrous sodium carbonate and 5.5 g of beryl frit. I melted the two together until formation of CO2 stopped, it took about 30
minutes at yellow heat. Then the cooled material was put in 100 ml of cold water and boiled to dissolve a part of it. Then 40 ml of 30% HCl was added
and boilled until only a few grams of precipitate on the bottom. It was filtered and boiled down to give very crude beryllium chloride. Theoretical
purity is 15% beryllium chloride, the yield was 5g.
|
Huh? On this occasion you don't appear to have separated to Be and Al? Your chloride is realyy (Al,Be) chloride? Or am I misunderstanding you?
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
It is Be, Al, and Na chloride, the Na could be easily removed tough. I keep the crude product until I get a good amount of it, then I will purify it.
I may try solvent extraction, or dissolve the Al and Be chloride with methanol, boil it down and react it with H2SO4 and ammonia to precipitate Al,
filter and boil down to get the beryllium sulphate.
I never asked for this.
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
I see.
Is your frit crushable/grindable? Down to powder? That would increase 'reactivity' enormously...
Another thing that might help with the separation is that AlCl3 is basically insoluble in conc. HCl. I've seen it precipitate with my own eyes: boiled
down an AlCl3 solution a lot, cooled, then added excess of 36 % HCl; white AlCl3 hydrated dropped out. But I don't know about BeCl2 behaviour in these
circumstances.
Keep it up.
|
|
plante1999
International Hazard
   
Posts: 1936
Registered: 27-12-2010
Member Is Offline
Mood: Mad as a hatter
|
|
Yes, my frit is crush-able, however my mortar broken recently. I just read something very interesting in parson book of beryllium chemistry, and
hopefully soon I will have all the reagent I need. Here is the idea:
A weight of beryl frit is mixed with it own weight of potassium hydroxide, and melted to a glass. The mix is covered with water, and slightly more
than stochiometric amount of conc. sulphuric acid is added, a gelatinous mass is formed. The mix is heated until it is dry and fuming. The dry product
is leached, and the potassium alum is precipitated by cooling. The purified beryllium sulphate is purified with other processes, but I would probably
only dry the filtrate to get the crude purified beryllium salt.
I only need to get potassium hydroxide and I should be ready to try.
I never asked for this.
|
|
blogfast25
International Hazard
   
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by plante1999  | Yes, my frit is crush-able, however my mortar broken recently. I just read something very interesting in parson book of beryllium chemistry, and
hopefully soon I will have all the reagent I need. Here is the idea:
A weight of beryl frit is mixed with it own weight of potassium hydroxide, and melted to a glass. The mix is covered with water, and slightly more
than stochiometric amount of conc. sulphuric acid is added, a gelatinous mass is formed. The mix is heated until it is dry and fuming. The dry product
is leached, and the potassium alum is precipitated by cooling. The purified beryllium sulphate is purified with other processes, but I would probably
only dry the filtrate to get the crude purified beryllium salt.
I only need to get potassium hydroxide and I should be ready to try. |
That's a variant on previous, really: 'break' the chemical structure of the beryl first by turning it into silicates/beryllate/aluminates. K alaum is
somewhat more soluble in the cold than NH4 alum, IIRW.
|
|