Potassium from K2CO3 + Mg lathings
On Youtube I found this video of some German guys making a kilo (!) of potassium metal.
https://youtu.be/FPjpXiZ1rSY
It looks amazing, although safety measures are not always observed.
I don't have these professionally made equipment, but I tried it with my humble stainless steel retort doing the same (but not a kilo !).
I heated 13g K2CO3 + 7g Mg lathings to about 1000 C in a propane furnace and after five minutes I captured 3.6g of potassium metal in an oil bath.
Even simpler than using KOH.



|
|
Sir_Gawain
Hazard to Others
 
Posts: 493
Registered: 12-10-2022
Location: [REDACTED]
Member Is Offline
Mood: Still in 2022
|
|
Fascinating! This does seem to be the easiest way to make potassium - I wonder if it would work with sodium.
“Alchemy is trying to turn things yellow; chemistry is trying to avoid things turning yellow.” -Tom deP.
|
|
chloric1
International Hazard
   
Posts: 1159
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
You know, I think it would be easier to get potassium carbonate to an anhydrous state. Second it has been shown magnesium reduces carbon dioxide as
well as potassium oxide and more than likely sodium oxide. BTW, where IS the carbon soot? Is the carbon dioxide being reduced or off gassed by
displacement?
Fellow molecular manipulator
|
|
metalresearcher
National Hazard
  
Posts: 790
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
When I opened the retort after cooling, there was carbon powder in the upper section of the retort.
Before I heated the K2CO3 to remove any moisture, but it is far easier than from KOH.
[Edited on 2024-9-6 by metalresearcher]
|
|
clearly_not_atara
International Hazard
   
Posts: 2827
Registered: 3-11-2013
Member Is Offline
Mood: Big
|
|
Awesome find!
|
|
metalresearcher
National Hazard
  
Posts: 790
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
And now I made sodium using NaOH prills with aluminum lathings and I got Na metal ! I used the same method: distilling using a stainless steel retort
ending in a jar with mineral oil which did capture some small balls of Na metal.
|
|
Precipitates
Hazard to Others
 
Posts: 154
Registered: 4-12-2023
Location: SE Asia
Member Is Offline
Mood: Acid hungry
|
|
That's amazing! Aluminium is much more accessible than magnesium.
Sodium from supermarket supplies! 
|
|
Random
International Hazard
   
Posts: 1120
Registered: 7-5-2010
Location: In ur closet
Member Is Offline
Mood: Energetic
|
|
Magnesium can be obtained from KUM pencil Sharpener
Edit
There was this Menthol Procedure
[Edited on 27-9-2024 by Random]
|
|