Conure
Hazard to Self
**




Posts: 53
Registered: 6-2-2023
Location: Schweden
Member Is Offline


[*] posted on 22-6-2024 at 10:02
Good way to thermally decompose ammonium molybdate?


I'm trying to make MoO3. I tried putting some ammonium molybdate in a steel vessel over a burner. The temp from the red hot bottom of the vessel is barely enough to turn the white powder into yellow MoO3. It requires lots of tedious stirring, otherwise it just goes from white to dull green. Is there a better method? Do I need a furnace, a lab oven or a powerful hot plate?

[Edited on 22-6-2024 by Conure]

[Edited on 22-6-2024 by Conure]




Fire is good. Fire is life.
View user's profile View All Posts By User
EF2000
Hazard to Others
***




Posts: 153
Registered: 10-5-2023
Location: The Steppes
Member Is Offline

Mood: Taste testing the Tonka fuel

[*] posted on 22-6-2024 at 10:41


Brauer's Handbook of Preparative Inorganic Chemistry recommends first reacting ammonium molybdate with nitric acid (maybe other reasonably strong acids can be used), then decomposing resulting molybdic acid (drying hydrated molybdenum trioxide) at about 150 °C for 16-20 hours: page 1412



Wroom wroom
"The practice of pouring yourself alcohol from a rocket fuel tank is to be strongly condemned encouraged"
-R-1 User's Guide
View user's profile View All Posts By User
Bedlasky
International Hazard
*****




Posts: 1241
Registered: 15-4-2019
Location: Period 5, group 6
Member Is Offline

Mood: Volatile

[*] posted on 22-6-2024 at 11:08


When I did decomposition of ammonium heptamolybdate, the resulting MoO3 always turned blue, indicating some MoO(3-x) contamination. I once saw jar with ammonium molybdate which had slightly blue hue. I look in to some papers and according to their analysis, decomposition in air should make pure MoO3 because of oxidizing power of O2. I did decomposition on hot plate, so maybe lower temperature favor uncomplete decomposition and partial reduction???? Who knows. For what purpose do you need MoO3?

https://core.ac.uk/download/pdf/42943961.pdf

[Edited on 22-6-2024 by Bedlasky]
View user's profile View All Posts By User
Conure
Hazard to Self
**




Posts: 53
Registered: 6-2-2023
Location: Schweden
Member Is Offline


[*] posted on 22-6-2024 at 12:01


Quote: Originally posted by Bedlasky  
When I did decomposition of ammonium heptamolybdate, the resulting MoO3 always turned blue,
...
For what purpose do you need MoO3?

https://core.ac.uk/download/pdf/42943961.pdf

[Edited on 22-6-2024 by Bedlasky]

It sometimes turn blue-black if the temp is not high enough. I get black spots in my powder.

I want to do thermitic reactions with MoO3 because it seems like a good alternative to Fe2O3, especially if with more exotic fuels. I have bought MoO3 from onyxmet.com but the purity keeps going down, my last order was dull green with garbage performance. And the price keeps increasing.




Fire is good. Fire is life.
View user's profile View All Posts By User
Conure
Hazard to Self
**




Posts: 53
Registered: 6-2-2023
Location: Schweden
Member Is Offline


[*] posted on 22-6-2024 at 12:03


Quote: Originally posted by EF2000  
Brauer's Handbook of Preparative Inorganic Chemistry recommends first reacting ammonium molybdate with nitric acid (maybe other reasonably strong acids can be used), then decomposing resulting molybdic acid (drying hydrated molybdenum trioxide) at about 150 °C for 16-20 hours: page 1412

Using molybdic acid is just as tiresome, I have tested. It requires high temp.




Fire is good. Fire is life.