Author: Subject: Don't ballmill magnesium.
Chemgineer
Hazard to Others
***




Posts: 216
Registered: 25-5-2021
Member Is Offline


[*] posted on 5-9-2022 at 08:02
Don't ballmill magnesium.


I've been ball milling magnesium to a 200 mesh powder without issue, i'm using a rubber container and ceramic media. However last week I opened the container and tried to see if it was fine enough for my mesh. It wasn't quite ready so I poured it back in and started it milling again.

I don't know quite know how it happened but about 2-3 minutes later it detonated and blew the end off my mill container, filled the area with thick smoke and started a small fire! Everything turned out ok and the fire went out with some water.

I think the lesson is that magnesium powder is hazardous and ball milling it is likely to result in an incident eventually.
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3032
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 5-9-2022 at 09:51


You should use some mineral oil when milling it. This is already adviced when milling aluminium, but with magnesium it is even more important.
View user's profile View All Posts By User
Chemgineer
Hazard to Others
***




Posts: 216
Registered: 25-5-2021
Member Is Offline


[*] posted on 5-9-2022 at 12:02


Good advice however I suppose it adds a solvent step to remove the oil afterwards, also I expect the lubrication slows down to milling?
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3032
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 5-9-2022 at 13:52


Both true, but at least your ballmill won't explode and start a fire.
View user's profile View All Posts By User
arkoma
Redneck Overlord
*******




Posts: 1763
Registered: 3-2-2014
Location: On a Big Blue Marble hurtling through space
Member Is Offline

Mood: украї́нська

[*] posted on 5-9-2022 at 23:29


Water might not be my first choice for possibly burning Magnesium.



"We believe the knowledge and cultural heritage of mankind should be accessible to all people around the world, regardless of their wealth, social status, nationality, citizenship, etc" z-lib

View user's profile View All Posts By User
Rainwater
National Hazard
****




Posts: 949
Registered: 22-12-2021
Member Is Offline

Mood: Break'n glass & kick'n a's

[*] posted on 6-9-2022 at 03:34


Quote: Originally posted by arkoma  
Water might not be my first choice for possibly burning Magnesium.

I second this!!!

Even a class 'ABC' extinguisher can add fuel to a magnesium fire, and many other combustible metals. If I remember correctly a class 'D' is used.
Table salt is another good option but be prepared for the possibility of chlorine gas.
Acid-washed sand and time are good methods to deal with most metal fires

I once got the idea to use an inert atmosphere of "party balloon helium" just to find out that it was roughly 40% He and 60% air. After the fire, I had some nice green rocks in my mill.

Stay safe.




"You can't do that" - challenge accepted
View user's profile View All Posts By User
BromicAcid
International Hazard
*****




Posts: 3254
Registered: 13-7-2003
Location: Wisconsin
Member Is Offline

Mood: Rock n' Roll

[*] posted on 6-9-2022 at 13:47


On the one hand, magnesium can form a nitride so finely divided magnesium could potentially still have issues in N2. On the other hand, it's nowhere near as prone to forming the nitride as lithium is: Case in point - Grignards are routinely run under nitrogen.



Shamelessly plugging my attempts at writing fiction: http://www.robvincent.org
View user's profile Visit user's homepage View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 7-9-2022 at 10:42


The explosive properties of magnesium are well documented.
At least you didn't have it fine enough to get a UV flash burn from the explosion.

I always open the container and let it sit for bit every 8 hours or so.
If your ball mill is more aggressive I would suggest a more frequent cycle.
This give the exposed fresh surfaces a chance to oxidize in a more controlled manner.

Some good charcoal (1%) is also useful in coating the surface and won't interfere with most pyrotechnic uses like a solvent might. After all your mix is probably going to contain charcoal anyway.

For a grignard you probably don't want the powder that fine. It will make generating the reagent too energetic. Of course grignards are finicky and you may know the material you are working with better than we would.
View user's profile View All Posts By User
Mateo_swe
National Hazard
****




Posts: 548
Registered: 24-8-2019
Location: Within EU
Member Is Offline


[*] posted on 16-10-2022 at 10:13


Wouldnt an oxygen free environment be the best for preventing an explosion?
It wouldnt be the easiest to make in a ball-mill jar but maybe one can just fill the jar with argon gas and close it (as argon is heavier than air)?
The jar needs to be air thight and not let any oxygen in.
Or wouldnt that work?
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 16-10-2022 at 10:45


How do you plan on emptying the mill?



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Mateo_swe
National Hazard
****




Posts: 548
Registered: 24-8-2019
Location: Within EU
Member Is Offline


[*] posted on 26-10-2022 at 02:54


Just open the mill jar after it has been standing a while so fine dust settles.
Isnt the danger when the milling action is going on and thus might create sparks or elevated temps?
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 26-10-2022 at 03:34


Reactive metals like magnesium and aluminum has a protective oxide layer that prevents further reactions with air. Milling strips off this layer, and the heat produced when it reforms can be enough to ignite fine powders.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Mateo_swe
National Hazard
****




Posts: 548
Registered: 24-8-2019
Location: Within EU
Member Is Offline


[*] posted on 30-10-2022 at 01:16


OK, how would you suggest doing it then?
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3032
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 30-10-2022 at 01:26


Quote: Originally posted by Tsjerk  
You should use some mineral oil when milling it. This is already adviced when milling aluminium, but with magnesium it is even more important.
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 30-10-2022 at 01:31


The general consensus is to open the jar frequently to reform the oxide layer (see macckones answer in this thread). Sadly I can't give you any more detailed advice as I haven't tried milling reactive powders. But I'm sure there are older threads on the topic.