[*] posted on 15-5-2006 at 08:19
Oxidizing CO using KMnO4


Hoping someone here can help me out with this:
I'm going to be heating a 1-atm lab furnace to approximately 1260C to melt some pieces of volcanic glass, but I need to keep the samples in a constant flow of CO-CO2 gas to prevent oxidation. Rather than just venting the CO-CO2, we're going to bubble it through a solution of KMnO4 to oxidize the CO to CO2 before venting it out the fume hood.

Anyone have any experience doing this? I'd appreciate any input-- thanks!
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 15-5-2006 at 10:51


I don't think that reaction's fast enough to be any use. If it were then gas analysis wouldn't mess about with solutions of copper (I) chloride in HCl or ammonia as a CO sorbent .

[Edited on 15-5-2006 by unionised]
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 15-5-2006 at 18:53


Just run it through a burner. CO burns quite nicely in air.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 16-5-2006 at 11:16


A fine solution but be careful when setting up- you don't want the flame to flash back into the reaction vessel.
Is there a good reason to add CO? Just using CO2 would be a lot less hazardous.
View user's profile View All Posts By User
volcanocowperson
Harmless
*




Posts: 2
Registered: 13-1-2006
Member Is Offline

Mood: No Mood

[*] posted on 16-5-2006 at 12:15


Hmm, I think I did a poor job explaining this-- sorry :)

The sample (pieces of volcanic glass) are going to be inside of a ceramic tube. Around the middle of the ceramic tube is a furnace-- so there's no flame anywhere, and the top and bottom of the ceramic tube are sticking out in contact with air.

But both ends of the ceramic tube are sealed-- gas flows in from the bottom (at room temperature), and out through the top (considerably warmer than room temperature, I'd imagine). We're using CO & CO2 to maintain the oxygen fugacity (partial pressure) such that my samples don't oxidize (in "normal" air at these temperatures, the samples would oxidize).

So we have gas flowing out of the ceramic tube, and it's a mix of CO & CO2-- rather than venting this straight out, we're planning to have it bubble through an Erlenmeyer with KMnO4 and water in it-- in theory, this gets rid of the CO (and our Environmental Safety people are happy).

My concern is that I'm not sure of the KMnO4 to water ratio, nor am I clear on how fast this reaction takes place (and thus, what volumes of gas flow I can use here).

Sorry for being unclear the first time around :)
View user's profile View All Posts By User
garage chemist
chemical wizard
*****




Posts: 1803
Registered: 16-8-2004
Location: Germany
Member Is Offline

Mood: No Mood

[*] posted on 16-5-2006 at 12:31


KMnO4 does not work, at least not fast enough.
Also, the manganese (heavy metal) waste from the KMnO4 is much more detrimental to the environment than some CO.
The environmental safety people obviously didn't think their idea through.

If you want to get rid of the CO, feed it into the air intake of a bunsen burner. That would be the best and most environmentally friendly method.
You wouldn' have to worry about flashback of the flame, since you have no oxygen in the furnace.




www.versuchschemie.de
Das aktivste deutsche Chemieforum!
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 17-5-2006 at 10:01


Carbon monoxide is quite capable of killing you in less time than it would take to safely purge the air from the apparatus if you get the set up wrong.
The oxygen fugacity in clean CO2 is practically nil.
If you really need the CO to act as a reductant you might want to think about generating it in situ by putting carbon in the furnace as well as the sample. Run CO2 through it cold until there's no air left, then heat the furnace so the C reduces the CO2 to CO and the sample melts in a reducing atmosphere. Switch off the furnace and let it cool with the CO2 still running.
That way you don't generate CO any more of the time than you need.

In any event, KMnO4 simply won't work. You could try I2O5, but really just venting the stuff out of the window is the best bet- it's simple and doesn't have any complicated bits to fail.
View user's profile View All Posts By User
The_Davster
A pnictogen
*******




Posts: 2861
Registered: 18-11-2003
Member Is Offline

Mood: .

[*] posted on 17-5-2006 at 15:31


Why not just run argon through instead? It keeps molten titanium unoxidized when I arc melt it.



View user's profile View All Posts By User
midnite13
Harmless
*




Posts: 3
Registered: 7-4-2006
Member Is Offline

Mood: Fascinated

[*] posted on 18-5-2006 at 14:17


Quote:
Originally posted by volcanocowperson
I'm going to be heating a 1-atm lab furnace to approximately 1260C to melt some pieces of volcanic glass

Hello, I just have a really newbie question pertaining to your lab.

What exactly is a 1-atm lab furnace? If you're going to be heating it to 1530K, according to Gay-Lussacs Law (Pi/Ti = Pf/Tf), wouldn't the pressure of the lab furnance change?

Sorry for the newbie question (=
View user's profile View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 18-5-2006 at 23:40


Er, yeah, the gas expands, there is less density when heated. It's not hermetically sealed.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
I am a fish
undersea enforcer
****




Posts: 600
Registered: 16-1-2003
Location: Bath, United Kingdom
Member Is Offline

Mood: Ichthyoidal

[*] posted on 27-5-2006 at 05:45


Quote:
Originally posted by garage chemist
...feed it into the air intake of a bunsen burner...


That wouldn't be the best method, as the flow rate of CO would affect the stoichiometry of the flame. CO is highly inflammable, and so it would be better to merely use the burner as a pilot light.




1f `/0u (4|\\| |234d 7|-|15, `/0u |234||`/ |\\|33d 70 937 0u7 /\\/\\0|23.
View user's profile Visit user's homepage View All Posts By User
The_Davster
A pnictogen
*******




Posts: 2861
Registered: 18-11-2003
Member Is Offline

Mood: .

[*] posted on 12-6-2006 at 16:58


From: Chemistry of the Elements by Greenwood
"I2O5 is notable in being one of the few chemicals that will oxidize CO rapidly and completly at room temperature
5CO + I2O5-->I2 + 5CO2
"




View user's profile View All Posts By User