Author: Subject: K2CO3 / KOH from Wood ashes ?
metalresearcher
National Hazard
****




Posts: 745
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 7-2-2021 at 08:42
K2CO3 / KOH from Wood ashes ?


I tried to extract soluble salts from wood ash.
I filled one third bucket with ashes from burnt beech + oak logs in my woodstove, added 2 liters of water and let it stand for over an hour and shaked the bucket a little.
Then I decanted off most liquid which I filtered through a coffee filter and a blob of Kaowool in the stem of the funnel (replacement for cotton which I don't have as it is as inert) to prevent tearing the filter when pouring in as it is very vulnerable when wet.
A clear tea-like brownish liquid which was about 800ml and felt very slippery, so it is moderately basic.
The color is probably due to Fe3+ ions.
But now my question: how can I separate K+ ions from this liquid ?

[Edited on 2021-2-7 by metalresearcher]
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 7-2-2021 at 10:08


The brown colour is more likely to me "humic acid" and or caramel like stuff than Iron.
Fe(OH)3 is very insoluble, and the solution is basic.
Probably the best bet for "what to do next" is put the solution in a shallow tray (glass or plastic) and let the water evaporate.
If you have some hydrogen peroxide, it might be interesting to see if that bleaches the colour at all.
Since K2CO3 is hygroscopic, I don't think you will get crystals forming unless you heat it to drive off water.
If you boil off all the water then you can roast the product- that will degrade the organics to carbon which is insoluble.
It also gives you a chance to weigh the product.
You might decide there's not enough material to be worth doing anything with.

The most practical way to convert it to KOH is to add Ca(OH)2 to the potash.

https://pubs.acs.org/doi/pdf/10.1021/ie51398a020



View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 8-2-2021 at 06:08


After dissolving the ashes and filtering you evaporate to dryness followed by blowtorching of the residue to redheat or something then purification
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 8-2-2021 at 06:15


The Canadian chemist on YouTube did a video on it I think
View user's profile View All Posts By User
EverythingAl2O3
Hazard to Self
**




Posts: 51
Registered: 3-9-2019
Member Is Offline


[*] posted on 9-2-2021 at 07:48


Quote:

I tried to extract soluble salts from wood ash.
I filled one third bucket with ashes from burnt beech + oak logs in my woodstove, added 2 liters of water and let it stand for over an hour and shaked the bucket a little.
Then I decanted off most liquid which I filtered through a coffee filter and a blob of Kaowool in the stem of the funnel (replacement for cotton which I don't have as it is as inert) to prevent tearing the filter when pouring in as it is very vulnerable when wet.
A clear tea-like brownish liquid which was about 800ml and felt very slippery, so it is moderately basic.
The color is probably due to Fe3+ ions. But now my question: how can I separate K+ ions from this liquid ?


I did something like this for a liming agent for my garden but not to the degree of purity that you might be going for. Its actually pretty simple. The preliminary leaching gets most contaminants out because they are insoluble. If you want a really pure K2CO3 then you could take your solution and add dry ice or bubble CO2 into it. This will precipitate out any KAl(OH)4 that formed as Al(OH)3 or Al2O3 (papers I read on making Al2O3 disagreed) and any Ca(OH)2 in solution will precipitate out as CaCO3. Some K2CO3 can precipitate out at the beginning because it has pH dependent solubility and is competing with the remaining KOH, but it can be recovered by dissolving the precipitate mix in distilled water (CaCO3 and Al(OH)3 will not go back in).
Then if you want the K2CO3 back as KOH add Ca(OH)2.

This is where I stopped the purification process because the plants don't care too much about the source of base as long as it isn't Na. Depending on your location Na could be a large contaminant (if you live in an area where your soil is inherently basic pH 7-8.5 then Na is likely to be a big contaminant. If the soils are naturally acid then it should be negligible. Seeing as you burned beech and oak they likely originated from an acid soil) but the other significant contaminant will be CaCl2 salts. I have not worked on how to separate them. The brown is likely leftover organics like Unionised said. Likely leftover lignin or polyphenols which are quite thermally stable and if the fire did not have the right amount of air they would not oxidize. A blow torch should solve that issue if you have one.

[Edited on 9-2-2021 by EverythingAl2O3]
View user's profile View All Posts By User
Maurice VD 37
Hazard to Self
**




Posts: 66
Registered: 31-12-2018
Member Is Offline


[*] posted on 9-2-2021 at 13:29


The wood ashes have the following composition :
40 - 70 % CaCO3
5 - 10% K2CO3
5 - 10 % Na2CO3
5 - 10% MgCO3
2 - 19% MgCO3
2 - 20% SiO2
2 - 6% Ca3(PO4)2
1 - 4% Mg3(PO4)2
1 - 5% K2SO4
0 - 2% AlPO4
0 - 1% FePO4
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 745
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 10-2-2021 at 01:55


Quote: Originally posted by Maurice VD 37  
The wood ashes have the following composition :
40 - 70 % CaCO3
5 - 10% K2CO3
5 - 10 % Na2CO3
5 - 10% MgCO3
2 - 19% MgCO3

2 - 20% SiO2
2 - 6% Ca3(PO4)2
1 - 4% Mg3(PO4)2
1 - 5% K2SO4
0 - 2% AlPO4
0 - 1% FePO4


So much CaCO3 and MgCO3 ?
How did you determine this ?

I checked the pH of the filtered wood ash solution and it was rather basic: 12.5, so that can't contain so much CaCO3 and MgCO3.

Here a picture after boiling off the water from 200ml of solution, yield about 9 grams.


RX609656.JPG - 2MBRX609654.JPG - 2.5MB
View user's profile View All Posts By User
clearly_not_atara
International Hazard
*****




Posts: 2731
Registered: 3-11-2013
Member Is Offline

Mood: Big

[*] posted on 10-2-2021 at 07:56


I assume Maurice gave a literature composition for the solid ashes, not the leachings. There is usually plenty of calcium in wood ashes, but CaCO3 does not dissolve in water.



Quote: Originally posted by bnull  
you can always buy new equipment but can't buy new fingers.
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 10-2-2021 at 09:25


Quote: Originally posted by Maurice VD 37  
The wood ashes have the following composition :
40 - 70 % CaCO3
5 - 10% K2CO3
5 - 10 % Na2CO3
5 - 10% MgCO3
2 - 19% MgCO3
2 - 20% SiO2
2 - 6% Ca3(PO4)2
1 - 4% Mg3(PO4)2
1 - 5% K2SO4
0 - 2% AlPO4
0 - 1% FePO4


I'd not expect that much sodium.
View user's profile View All Posts By User
Maurice VD 37
Hazard to Self
**




Posts: 66
Registered: 31-12-2018
Member Is Offline


[*] posted on 10-2-2021 at 13:30


The analysis I have reported describe the composition of the solid ashes, before any leaching or treatment. The basicity of the solution is due to the carbonates of sodium and potassium. I have also been surprised about the amount of sodium.
View user's profile View All Posts By User
Plinius
Harmless
*




Posts: 4
Registered: 11-1-2021
Member Is Offline


[*] posted on 11-2-2021 at 05:21


When the solution is evaporated K2SO4 crystallizes out first. The amount of K2SO4 obtained is about 10% of the total amount of salts. The yield of K2CO3 I have obtained agrees with the analysis presented above.

I once read that ash from birch or beech is best. Ash from coniferous trees is not so good, why I do not know.
View user's profile View All Posts By User
Piroz
Harmless
*




Posts: 19
Registered: 15-12-2020
Location: Poland
Member Is Offline


[*] posted on 11-2-2021 at 15:50


Treating solution with CO2 is a great idea. I found that alcoholic fermentation is good source of CO2. So I decided to treat small portions of concentrated solution from wood ashes with carbon dioxide from carboy. Next the solution with crystalline precipiptation was collected in the bottle. Then I carefully left solution for slowly crystallisation in open containers and I found something interesting. The first crystals that grew were pillars- like(or needle- like). I'm sure that isn't carbonate or bicarbonate due to no generation of CO2 in reaction with acetic acid. Also the crystal shape doesn't looks like any sulfate, more looks like phosphate. After some time the second type of crystals (flat) starts to grow. It looks like potassium bicarbonate- they violently react with acetic acid to form CO2 and give lilac colour of flame. After heating in open flame it forms snowy-white compound, very hygroscopic (some particles made mess on the table after few minutes). However it also contains traces of sodium that give some yellow flame. Needle-like crystals also gives the yellow colour of flame but stronger so sodium content is higher.
I think that's the best way to get potassium carbonate from wood ash- by separation of potassium bicarbonate using slowly crystallisation and then heating it to obtain carbonate.
I'm also not sure about first crystals that separates out on the bottom of bottle. I'll try to crystallise it after dissolve in water.

Edit: it looks like sodium occurs as sodium-potassium carbonate mix


Quote:

A Potassium sodium carbonate, K2CO3,Na2CO3,12H2O, is a constituent of vegetable ashes. At 35° C. it decomposes in accordance with the equation

3(K2CO3,Na2CO3,12H2O) = 2K2CO3 + K2CO3,3Na2CO3,10H2O + 26H2O.

The double carbonate thus generated decomposes at a temperature of about 130° C.


source: http://potassium.atomistry.com/potassium_sodium_carbonate.html

But I'm suprised that is 5 - 10 % of Na2CO3, it's large amount. It doesn't look like so much sodium.

WInemaking_carbonate.jpg - 477kB Solution_saturated_CO2.jpg - 200kB Crystallisation_in_open_containers.jpg - 299kB Two_types_of_crystals.jpg - 279kB Unknown_crystals.jpg - 466kB Bicarbonate1.jpg - 243kB Bicarbonate2.jpg - 296kB Lilac_flame.jpg - 467kB

[Edited on 11-2-2021 by Piroz]

[Edited on 12-2-2021 by Piroz]

[Edited on 12-2-2021 by Piroz]
View user's profile View All Posts By User
Plinius
Harmless
*




Posts: 4
Registered: 11-1-2021
Member Is Offline


[*] posted on 13-2-2021 at 06:08


I once read a description of potash production from - I think - the 19th century. It was mentioned that if the wet ashes were stored for some weeks in contact with air, the yield of K2CO3 was increased. The reason given was that the carbon dioxide absorbed from the air decomposed silicates present in the ash.

I have never seen crystals which look like needles when making potash.
View user's profile View All Posts By User