Cleaning copper chromite from frit glass


I made some copper chromite and used the frit to pull water after the acedic acid wash.

I was able to clean the frit surface with soap and water and although it functional it still has some gray stain.

Any suggestions on what to try? HCL acid doesn't touch it and I tried sulphuric acid drain cleaner (pure is on the way) and that didn't it touch it either.

Those are the only things I have tried so far. I plan to try Chromic Acid next but that will be a few days.
View user's profile View All Posts By User
DavidJR
National Hazard
****




Posts: 908
Registered: 1-1-2018
Location: Scotland
Member Is Offline

Mood: Tired

[*] posted on 17-12-2019 at 15:43


Try soaking in a solution of EDTA disodium.
View user's profile View All Posts By User
rockyit98
Hazard to Others
***




Posts: 283
Registered: 12-4-2019
Location: The Known Universe
Member Is Offline

Mood: no mood is a good mood

[*] posted on 17-12-2019 at 20:25


what about con. HNO3? maybe it will oxidize it back to copper chromate .i guess con. Ammonia can be used to dissolve copper chromate if good luck would have it even copper chromite itself.



"A mind is a terrible thing to lose"-Meisner
View user's profile View All Posts By User
jderimig
Harmless
*




Posts: 10
Registered: 25-11-2019
Member Is Offline


[*] posted on 18-12-2019 at 06:08


Quote: Originally posted by DavidJR  
Try soaking in a solution of EDTA disodium.


That is on my list to try, trying to source some locally.
View user's profile View All Posts By User
jderimig
Harmless
*




Posts: 10
Registered: 25-11-2019
Member Is Offline


[*] posted on 18-12-2019 at 06:12


Quote: Originally posted by rockyit98  
what about con. HNO3? maybe it will oxidize it back to copper chromate .i guess con. Ammonia can be used to dissolve copper chromate if good luck would have it even copper chromite itself.


I have trying 30% aqueous ammonia and there didn't seem to be a reaction. I will try some HNO3 after I distill some.

I have some KMnO4 on the way as I found in another thread that it might convert Cr2O3 so its soluable in HCL or HNO3. So maybe if it acts on Cr3O3 it might work on CuCr2O5?

Keep the suggestions coming.
View user's profile View All Posts By User
DavidJR
National Hazard
****




Posts: 908
Registered: 1-1-2018
Location: Scotland
Member Is Offline

Mood: Tired

[*] posted on 18-12-2019 at 07:06


In future don't use frits for filtering anything which you don't know how to dissolve again later. It can sometimes be completely impossible to get them clean again.

A traditional Buchner funnel with filter paper does not have this problem (because the filter paper is disposable).
View user's profile View All Posts By User
jderimig
Harmless
*




Posts: 10
Registered: 25-11-2019
Member Is Offline


[*] posted on 18-12-2019 at 07:28


Quote: Originally posted by DavidJR  
In future don't use frits for filtering anything which you don't know how to dissolve again later. It can sometimes be completely impossible to get them clean again.

A traditional Buchner funnel with filter paper does not have this problem (because the filter paper is disposable).


Yup, lesson learned. I saw the method for producing CuCr in a video and he used a frit filter in the final step that was white as the driven snow. So I figured he'd done this before and cleaning the frit would not be a space shot.
View user's profile View All Posts By User
PirateDocBrown
National Hazard
****




Posts: 570
Registered: 27-11-2016
Location: Minnesota
Member Is Offline

Mood: No Mood

[*] posted on 18-12-2019 at 08:17


I often place a circle of filter paper on top of the frit, you get a double filtering effect, and much crap is kept out of the frit.



Phlogiston manufacturer/supplier.

For all your phlogiston needs.
View user's profile View All Posts By User
jderimig
Harmless
*




Posts: 10
Registered: 25-11-2019
Member Is Offline


[*] posted on 23-12-2019 at 11:40


Update: Think I found a solution.

Soak frit in solution of KMn04 (I did overnight).
Then soak in concentrated HCL. Seems to be doing the trick.
View user's profile View All Posts By User
SuperOxide
Hazard to Others
***




Posts: 486
Registered: 24-7-2019
Location: Devils Anus
Member Is Offline


[*] posted on 1-8-2021 at 15:53


Quote: Originally posted by jderimig  
Update: Think I found a solution.

Soak frit in solution of KMn04 (I did overnight).
Then soak in concentrated HCL. Seems to be doing the trick.


Sorry to bump an old thread - but can you confirm if this is a solution or not? I plan on doing this synth soon, and am planning the proper cleanup (including of the frit).

Thanks.




View user's profile View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 3-8-2021 at 06:53


yes, that will work for this combo.
bleach should work as well in place of KMnO4.
But bleach is going to generate some chlorine gas.
sodium chlorate might work better but bleach is more accessible.
View user's profile View All Posts By User
SuperOxide
Hazard to Others
***




Posts: 486
Registered: 24-7-2019
Location: Devils Anus
Member Is Offline


[*] posted on 15-8-2021 at 09:56


Quote: Originally posted by macckone  
yes, that will work for this combo.
bleach should work as well in place of KMnO4.
But bleach is going to generate some chlorine gas.
sodium chlorate might work better but bleach is more accessible.


I have some EDTA Disodium Salt Dihydrate that I purchased just for this test. And I dissolved some into solution, and added some copper chromite to it and let it sit for some time. The solution went from clear, to green, to blue. And there's still some black copper chromite at the bottom.
.

I added about equal quantities of the EDTA disodium and copper chromite (one scoop of each), but now that I think about it, the EDTA disodium salt molecule is bigger than a molecule of copper chromite, right? So maybe equal volumes isn't right, I need to do a 1-1 molar ratio (at least).

I'm going to test out how well free EDTA acid works to compare (as opposed to the disodium salt).
It seems I can get the free EDTA acid by adding HCl to a solution of the EDTA disodium salt, which will make free EDTA and sodium chloride. EDTA is much less soluble in water than the disodium salt or sodium chloride.
I added 3g of the disodium salt to some distilled water in a test tube, then once dissolved, added some conc HCl, and eventually a lot of EDTA fell out of solution :-)

here are some more pics of that little pilot synth.

It seems that free EDTA may be more useful than the EDTA disodium salt, so I'm going to make some in a larger run - which I'm doing now (processing 80g of the disodium dihydrate salt).

If anyones interested in a comparison between the two forms of EDTA (in terms of cleaning up metals), then lmk and I'll share the results :-)

Edit: Now that I think about it though... The free EDTA is much less soluble in water, so maybe it wouldn't be as easy to use... hmm. Oh well. Still fun to test it out.

[Edited on 16-8-2021 by SuperOxide]




View user's profile View All Posts By User
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 17-8-2021 at 08:43


Quote: Originally posted by macckone  
yes, that will work for this combo.
bleach should work as well in place of KMnO4.
But bleach is going to generate some chlorine gas.
sodium chlorate might work better but bleach is more accessible.


Better, first add vinegar to the dilute aqueous NaOCl/NaCl (aka, bleach). This creates HOCl which behaves like H2O2 in a fenton-type reaction. The Chromium oxidation state increases and yes, in the presence of NaCl, expect some Chlorine liberation as well.

Do not leave the mix sitting around as you could get a nasty smelling (and problematic) chloro-acetate in time.

Safer, but perhaps less effective, use a mix of Chlorine bleach and Baking Soda. Again, HOCl at work but no chloro-organics!

[Edited on 17-8-2021 by AJKOER]
View user's profile View All Posts By User

  Go To Top