Author: Subject: How to repair a thermocouple?
Pumukli
National Hazard
****




Posts: 708
Registered: 2-3-2014
Location: EU
Member Is Offline

Mood: No Mood

[*] posted on 6-1-2019 at 10:38
How to repair a thermocouple?


I have a thermocouple at the end of a meter long wire-pair, (thermometer sensor.) Unfortunately one of the wires broke at the small junction globule. I'd like to repair it but don't know how to proceed.
I thought of discharging a bigger electrolytic capacitor into this junction and make it remelt again. (But how much joules?)

I know the couple is cheap (USD 1, including shipping and handling, maybe), but I don't want to bin it yet.

Had anyone repaird a thing like this?
View user's profile View All Posts By User
Sigmatropic
Hazard to Others
***




Posts: 307
Registered: 29-1-2017
Member Is Offline

Mood: No Mood

[*] posted on 6-1-2019 at 10:40


Sand the wires and wrap 'm together. Worked fine in my case.
View user's profile View All Posts By User
happyfooddance
National Hazard
****




Posts: 530
Registered: 9-11-2017
Location: Los Angeles, Ca.
Member Is Offline

Mood: No Mood

[*] posted on 6-1-2019 at 10:48


Yes, I did it similar to how you described, I welded it by discharging a capacitor from what I believe was a 12v power supply. I'm not sure the amount of energy discharged, but I varied it (by using a resistor), and it took a few (maybe 2 or 3) tries before I got a clean weld. I cleaned the pieces between tries and added a small amount of flux (probably a mix of dilute HCl, Zinc Chloride, and borax or tri-sodium phosphate).

There is a certain trick to getting the arc to form in the right spot, I'm not a welder or an expert, but for me the ends needed to be more parallel and less tip-to-tip, if that makes sense.
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 6-1-2019 at 10:57


If it's used for low temperature you can solder it.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
morganbw
National Hazard
****




Posts: 561
Registered: 23-11-2014
Member Is Offline

Mood: No Mood

[*] posted on 6-1-2019 at 11:11


Quote: Originally posted by Sigmatropic  
Sand the wires and wrap 'm together. Worked fine in my case.


Not the correct way but just twisting the wires at the junction often work remarkably well.
Just saying.

[Edited on 1/6/2019 by morganbw]
View user's profile View All Posts By User
Twospoons
International Hazard
*****




Posts: 1327
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline

Mood: A trace of hope...

[*] posted on 6-1-2019 at 11:35


I've used the arc from a neon sign transformer to make thermocouples. Melts a nice little ball on the end of the wire.
As has been said, soldering works too, though you need an aggressive flux such as ZnCl / HCl.




Helicopter: "helico" -> spiral, "pter" -> with wings
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 6-1-2019 at 13:02


In my experience twisting and soldering works fine without any special flux. At least for "single use" or non-critical applications. We routinely measured heat production in curing concrete, the TC was twisted&soldered with regular 50/50 flux core and embedded un-shielded into the wet concrete. This worked fine for at least a week.



We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
Twospoons
International Hazard
*****




Posts: 1327
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline

Mood: A trace of hope...

[*] posted on 6-1-2019 at 15:16


Your 50/50 solder probably does have an aggressive flux, given the usual application for that alloy is soldering pipes etc. This is different to 63/37 Sn/Pb used in electronics, which usually has a much milder flux, and in my experience doesn't work as well with nickel alloys.



Helicopter: "helico" -> spiral, "pter" -> with wings
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3727
Registered: 8-2-2015
Location: 3rd rock from the sun
Member Is Online


[*] posted on 6-1-2019 at 15:37


For temporary use twisting wires together works ok,
type J used in a lot of older equipment can be soldered,
I've never succesfully soldered type K




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
Ubya
International Hazard
*****




Posts: 1247
Registered: 23-11-2017
Location: Rome-Italy
Member Is Offline

Mood: I'm a maddo scientisto!!!

[*] posted on 6-1-2019 at 16:52


i don't think soldering would be a good idea, i mean a thermocouple works because when to different metals are in contact and are heated they generate a small electric potential, if you solder them with a random filler metal, the propriety of the probe would change right?




---------------------------------------------------------------------
feel free to correct my grammar, or any mistakes i make
---------------------------------------------------------------------
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1726
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 6-1-2019 at 18:02


My bad, I meant the standard fine electronics solder. I suspect it acted more like an adhesive, and that the electrical contact was formed by twisting the pair. Either way it performed flawlessly, even when suspended in concrete.

As for the TC a solder joint shouldn't affect the performance. The chromel-solder / solder-alumel dual couple would produce the same voltage difference as the standard chromel-alumel couple.




We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
DavidJR
National Hazard
****




Posts: 908
Registered: 1-1-2018
Location: Scotland
Member Is Offline

Mood: Tired

[*] posted on 6-1-2019 at 19:00


Solder may work but it most certainly will change the temperature/voltage curve of the thermocouple. It may, however, still operate acceptably well, but no guarantees.
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5128
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 7-1-2019 at 02:20


Quote: Originally posted by Ubya  
i don't think soldering would be a good idea, i mean a thermocouple works because when to different metals are in contact and are heated they generate a small electric potential, if you solder them with a random filler metal, the propriety of the probe would change right?

Odd as it seems, as long as all the soldered bits are at the same temperature, the solder does not affect the output voltage.
So, chromel, solder, alumel gives the same voltage as chromel, alumel. (provided that the alumel solder and solder chromel junctions are at the same temperature).

View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 765
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 7-1-2019 at 15:33



The soldering will work as long as you are measuring lowish temps. If you go near the melting temp. of the solder the junction will dissolve into the solder and things will not work. Brazing will work so long as you do not go near the melting temp. of the braze. If you go near the ....... (as with the solder above!)

Try to melt wires together. Not easy to do.