Lowest melting point alkali carbonate or alkali carbona eutectic
Dear Friends,
I hope this is the correct section for this. Recently I am researching the molten carbonate fuel cells. This type of fuel cells are the most robust
fuel cells with respect to CO poisoning. However their main disadvantage is they have to be heated to operating temperature (i.e. their melting point)
before they produce electricity. All alkali carbonates I am researching have high melting points. Consequently, I am looking for a low melting point
alkali carbonate or alkali carbonate eutectics. Any ideas? Regards.
|
|
BromicAcid
International Hazard
   
Posts: 3269
Registered: 13-7-2003
Location: Wisconsin
Member Is Offline
Mood: Rock n' Roll
|
|
2nd result on google searching "Molten Salt Database" was the hit I was looking for.
http://ras.material.tohoku.ac.jp/~molten/molten_ps_query1.ph...
Give it a shot.
|
|
akinmad
Hazard to Others
 
Posts: 245
Registered: 24-7-2003
Member Is Offline
Mood: No Mood
|
|
Thank you. I had previously visited that link but it does not give melting points (or am I missing something?). Regards
|
|
12AX7
Post Harlot
   
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
Pretty close, you wanted this.
http://ras.material.tohoku.ac.jp/~molten/molten_eut_query1.p...
I find:
System: KCl-K2CO3-Na2CO3, Mol %:42.5-43.3-18.1, Temp: 558 C
System: K2CO3-Na2CO3 , Mol %: 38.5-61.5, Temp: 695 C
System: K2CO3-Li2CO3-Na2CO3, Mol %: 26.8-42.5-30.6, Temp: 393 C
Tim
[Edited on 11-4-2005 by 12AX7]
|
|