Author: Subject: Making Potassium metal by distillation with Al and KOH
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 1-5-2018 at 00:12
Making Potassium metal by distillation with Al and KOH


I recently came across a video of distilling potassium by reducing KOH with Al powder, I was not aware that it was possible to use aluminium powder to do this, especially since magnesium did not work for codys lab, I, however also got this method to work very well with little difficulty, same as the video I used a CO2 cartridge with a copper tube for my reaction vessel, added 10g of KOH, dried with a gas torch and put in 3.5g of 200mesh Al powder (cheap one not flake or dark), my gas torch proved to be not big and hot enough so I put it in a simple blast furnace, this worked quickly and the potassium distilled over into a test-tube, the potassium seemed pure, no contamination aside from oxidation which is unavoidable without a inert gas, I got about 2g maybe. It passed all my tests: shiny and metallic when fresh, melts about 60*C, ignites and burns the recognizable potassium purple in water then explodes.
As I said I was not aware this reaction worked so any ideas are welcome, this seems like a very easy way to make potassium, easier than the catalyzed magnesium reduction (in my opinion), and also cheaper and more pure than this method but with sodium and KCl

The video came from Огненное ТВ and was called PREPARATION OF POTASSIUM AND SODIUM IN HOME CONDITIONS

link: https://www.youtube.com/watch?v=5JdPQucTjjg&t=6s

The picture is not that great if it came through, the test-tube had potassium coating the inside, and I have not had time to clean it up much.



31542656_531882910546444_5503354373339611136_n.jpg - 145kB
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6338
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 1-5-2018 at 02:39


Well, I am impressed. This is a good result.
I have seen this video before -- I subscribe to this channel. But I watch few videos since I don't speak Russian.

It sounds like it is worth giving this a crack myself.
Thanks for highlighting this method for us.




View user's profile View All Posts By User
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 1-5-2018 at 08:33


Possible reaction path:

3 [ 2 KOH + Heat --> K2O + H2O ]

Al + 3 H2O + Heat --> Al(OH)3 + 3/2 H2

3/2 [ H2 + K2O = 2 K (g) + H2O ]

3/2 [ K2O + H2O --> 2 KOH ]

Implied net reaction for the above:

6 KOH + Al + Heat --> Al(OH)3 + 3 K (g) + 3 KOH

or simply:

3 KOH + Al + Heat --> Al(OH)3 + 3 K (g)

[Edited on 1-5-2018 by AJKOER]
View user's profile View All Posts By User
Sigmatropic
Hazard to Others
***




Posts: 307
Registered: 29-1-2017
Member Is Offline

Mood: No Mood

[*] posted on 1-5-2018 at 09:12


Good speculation AKJOER, except that Al(OH)3 will dehydrate into aluminium oxide, releasing water. Which will feed back into the reaction, chewing up more Al under the formation of hydrogen. Also why exactly do you think hydrogen reacts with potassium oxide to form water and elemental potassium. It is not only strongly endothermic but also uphill with regard to the oxidation potential.
I would speculate this reaction is better described by:
6 KOH + 2 Al --> K2Al2O4 + 2 K2O + 3 H2
Seeing that K2Al2O4 is comparable to the complex K2O*Al2O3 I would argue the equations below are equivalent.
2KOH - - > K2O + H2O
3 H2O + 2 Al --> Al2O3 + 3 H2

To arrive at potassium metal a thermitic reaction between K2O and Al. Probably also ending in K2Al2O4.
4K2O + Al --> 2 K + K2Al2O4
View user's profile View All Posts By User
VSEPR_VOID
National Hazard
****




Posts: 719
Registered: 1-9-2017
Member Is Offline

Mood: Fullerenes

[*] posted on 1-5-2018 at 09:20


Are there any high temperature desiccants that can be used to absorb any water produced by the thermal decomposition of the aluminium hydroxide?

I am not on a network that permits me to go to ebay and see, but could you use your method to produce cheap potassium metal and sell it? KOH and Al powder are dirt cheap.

[Edited on 1-5-2018 by VSEPR_VOID]




Within cells interlinked
Within cells interlinked
Within cells interlinked
View user's profile View All Posts By User
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 1-5-2018 at 17:22


I did some research, and per a source on the action of H2 on NaOH (which I think may parallel KOH), we have:

H2 + NaOH = NaH + H2O (see Eq 1 on page 2192)

and at 360 C :

NaH + Heat --> Na + 1/2 H2

Source: See 'Revisiting the Hydrogen Storage Behavior of the Na-O-H System' by Jianfeng Mao , et al., in Materials 2015, 8, 2191-2203; doi:10.3390/ma8052191 . Link to download file: https://www.mdpi.com/1996-1944/8/5/2191/pdf . To quote:

"The DTA profile for NaH shows one endothermic peak at ca. 360 °C, which can be assigned to the decomposition of NaH to Na metal and hydrogen."
--------------------------------------------------

Actually, in my opinion, the actual chemistry is likely a function of the highly anodic metal (like Mg, Zn, Al, Fe, Sn,.., see http://www.zygology.com/cms/upload_area/pdf/Zyg-Anodic-Index... where Zn and Al are the frequent cited sources of so called 'nascent hydrogen' with HCl) reacting with water as follows:

H2O = H+ + OH-

Al --> Al3+ + 3 e-

e- + H+ = .H = 1/2 H2 (as .H + .H = H2)

Hence, the cited Equation (1) above could actually be the net of the following reactions:

.H + OH- = e- + H2O = e-(aq) (see Eq 37 and Table 2 at https://pdfs.semanticscholar.org/d696/b35956e38351dd2eae6706... )

e- + .H = H- (see http://pubs.rsc.org/-/content/articlelanding/1966/tf/tf96662... )

Net of the two above:

2 .H + OH- = H- + H2O

or, seemingly (but not so at very high temperatures as H2 + Heat = .H + .H):

H2 + OH- = H- + H2O

Further:

H- + Heat --> .H + e- = 1/2 H2 + e- (as .H + .H = H2)

and:

e- + Na+ = Na

My point is if one is going to give credit to the hydrogen, and ignore the role of the highly anodic metal, it is really the mono-atomic hydrogen radical (.H formed courtesy of the anodic metal or high temperatures), or as historically sometimes referred to, in my estimation, as 'nascent' hydrogen. Here is a recent account of the surface chemistry of adsorbed .H on aluminum and applications, see https://books.google.com/books?id=1etfSdk55SYC&pg=PA817&... . This last reference per Equation (5) appears to support my reaction presentation in terms of 2 .H (which is adsorbed on an aluminum surface) and not H2, to quote:

" PbS + 2 .H = Pb + H2S (5) "

[Edited on 3-5-2018 by AJKOER]

[Edited on 3-5-2018 by AJKOER]
View user's profile View All Posts By User
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 1-5-2018 at 17:39


Thanks for the input, to add to it in practice not much water is produced, just slight condensation in the test-tube, so that's not a problem

VSEPR_VOID It is very cheap but laws and regulations in my country make it almost imossible to buy potassium let alone sell it, I had to wait 2 years for Al powder to be available.
View user's profile View All Posts By User
Foeskes
Hazard to Others
***




Posts: 156
Registered: 25-2-2017
Member Is Offline

Mood: No Mood

[*] posted on 2-5-2018 at 18:08


Cody used KCl not KOH. I'm pretty sure using KOH with magnesium would work but would be really violent and self sustaining. Like the Mg and NaOH reaction.
View user's profile View All Posts By User
Diachrynic
Hazard to Others
***




Posts: 226
Registered: 23-9-2017
Location: western spiral arm of the galaxy
Member Is Offline

Mood: zenosyne

[*] posted on 2-5-2018 at 20:55


This is great! How do you think it got? More than 1000 °C?



we apologize for the inconvenience
View user's profile View All Posts By User
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 2-5-2018 at 23:20


Diachrynic The potassium boils at 759*C so it would not be necessary to get to 1000*, also I used copper tubing to distill out the potassium so I couldn't let it get that hot, unfortunately when I attempted cesium a while ago the copper tubing did melt, just when I had something I couldn't afford to fail it did.

Just a photo of the reaction vessel, cost me about $4, no welding or brazing just a friction fit, so pretty much anyone could do it.
View user's profile View All Posts By User
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 2-5-2018 at 23:34


The photos didn't come through so here they are:


31764722_533356553732413_2092747657066840064_n.jpg - 50kB 31765967_533348360399899_4561561989146476544_n.jpg - 143kB
View user's profile View All Posts By User
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 8-5-2018 at 21:45


I just made a basic video on the process so thought I might mention it here, I have got almost exactly the same results twice in a row so it doesn't seem hard.

video: https://youtu.be/2ORTcQB8kOc
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6338
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 8-5-2018 at 21:55


Nice! Well done.
This looks like a reliable, efficient setup.




View user's profile View All Posts By User
VSEPR_VOID
National Hazard
****




Posts: 719
Registered: 1-9-2017
Member Is Offline

Mood: Fullerenes

[*] posted on 9-5-2018 at 01:51


What heat source did you use to get it to 1000C?



Within cells interlinked
Within cells interlinked
Within cells interlinked
View user's profile View All Posts By User
Yb(NO3)3
Harmless
*




Posts: 6
Registered: 30-4-2018
Member Is Offline

Mood: No Mood

[*] posted on 9-5-2018 at 11:42


I used wood as fuel for the furnace, it does burn through it very quickly but coal is too hot and can melt the copper tubing, I think charcoal briquettes would be probably be better.
View user's profile View All Posts By User
Foeskes
Hazard to Others
***




Posts: 156
Registered: 25-2-2017
Member Is Offline

Mood: No Mood

[*] posted on 24-6-2018 at 07:14


I decided to try it out and it worked! (I used a small butane brazing torch by kovea in a flower pot lined with sand and plaster.$
I got 3 spheres of potassium and when added to water it burns with a nice purple flame.
I used a co2 canister with a high pressure rated brass tube (just pushed in no screws)
For some reason the zinc on the receiving end of the apparatus disappeared leaving only copper.
And sone wired black chunks were in the oil with the K, it reacts with water violently while sinking and seems to produce CuO and is brittle. I assume it's a mix of potassium and copper oxide or some kind of cuperate from burning potassium.
The main problem I have is before the potassium drops into oil it would stick to the tube and oxidize.
I put some butane in the container so ignore the bubbles.

image.jpeg - 481kB
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 24-6-2018 at 07:22


Sweet !



View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 759
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 14-10-2019 at 10:56
I tried, but to no avail


I used a welded steel retort (22mm OD) attached with a gas pipe coupling to a 12mm copper tube ending in a test tube with lamp (mineral) oil.
I first heated the KOH to 600 C to dry it and then let the lye (which is actually molten KOH) freeze and cool down and added the Al powder and tightened the screws very tightly. Then I heated the retort to 950 C (measured with an infrared contactless pyrometer), but it only bubbled slightly for less than a minute and after that nothing happened, even no bubbling. A few times I turned off the burner to check for leaks (which then should appear as white smoke) but no smoke was detected and when the flame was on, no purple/magenta coloring (the K+ ion color) of the flame took place.

But adding water in the opened retort afterwards resulted in a small explosion (so actually a very few K metal was in it), but why did it not evaporate, despite the retort temperature is well above the bp of K (768 C) ?


RX607538.JPG - 437kB




View user's profile View All Posts By User
elementcollector1
International Hazard
*****




Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline

Mood: Molten

[*] posted on 15-10-2019 at 07:40


Improper mixing, maybe? Though the aluminum would also be molten at that point...

What was your stoichiometry? Maybe you lost most of your K to aluminate and need more starting Al.




Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 759
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 15-10-2019 at 08:34


I used stabilized Al powder (3.5g) and 11g KOH of which is I guess 7-8 g real KOH, rest water.
Today I did another try, now with Mg turnings.
I let it run for about 20 minutes, as long as it bubbled in the test tube with the oil.

Here a video of yesterdays attempt with Al powder and after it today's attempt.

https://www.metallab.net/jwplayer/video.php?v=L2NsaXBzL0tPSC...

Afterwards there was some tiny amount of K in the retort, because when watering it, flames appeared (see video).


[Edited on 2019-10-15 by metalresearcher]




View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 16-10-2019 at 04:40


Koh is about 10%water until it's dried so 11g would be more like 9.9g koh
7-8 is a bit on the low side.
View user's profile View All Posts By User