Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
 Pages:  1  
Author: Subject: Electrochemical color passivation of stainless steel
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 28-2-2018 at 14:39
Electrochemical color passivation of stainless steel


I have been lately facinated with metal surface treatment methods....anodizing.....magnetite (black oxide)....parkerizing....and the tough task of producing iridescent light interference coatings on stainless alloys.
The straightforward anodizing of titanium proved to be very simple: just apply a dc voltage in the range of 5-120V across any conductive solution, connect the Ti detail to be colored as the anode and watch the colors develop as a function of applied potential difference.

DSCF1551.JPG - 249kB

Fig. 1 The iridescent blue interference layer produced on Ti substrate at about +27V dc in a saturated sodium bicarbonate water solution

Fascinating yet kind of boring.... :D

The black oxide or magnetite coating on ferrous alloys is usually applied by submerging the details in a hot caustic salt bath of concentrated lye and nitrate mixture at about 150C. A rather nasty and dangerous enterprise to conduct on the corner of your kitchen table, to be honest.
Fortunately there is a rather neutral bypass that delivers comparable results accompanied only by the threat of burning oneself with hot water....cooking up a batch of chicken soup is about as dangerous :D
Based on US3920486A
------------------------------------------------------------
Black oxide bath:

Ammoinum nitrate 10g/l
KClO3 150mg/l
Water balance
Optimum operating temperature 95-100C
------------------------------------------------------------

DSCF1519.JPG - 281kB
Fig. 2 Raw details machined out of mild steel



DSCF1521.JPG - 375kB
Fig. 3 Degreased with dishwashing detergent and submerged into the aforementioned bath composition at about 95C


DSCF1523.JPG - 286kB
Fig. 4 A full suspense filled 30 minutes of slow simmer later....



DSCF1526.JPG - 299kB DSCF1527.JPG - 243kB
Fig. 5 Fully magnetite coated details ready to be oiled and assembled

The simple and dirt cheap bath works really good and on a rather wide selection of ferrous alloys and also on high speed steels. The formed coating is very tough, uniform and resists mechanical scratching and the corrosive attack of a saturated sodium chloride solution even without being saturated with oil for a minimum of 24h.




DSCF1553.JPG - 300kB DSCF1559.JPG - 285kB DSCF1560.JPG - 266kB DSCF1562.JPG - 302kB
Fig. 6 Selection of different ferrous alloys coated in the aforementioned bath: High carbon steel detail (10.9 strength class threaded rod center), T1/P18 tool steel tap, utility knife blade SK-5 steel, ball bearing rim.
Working solutions....literally :)



But onwards....to the forced coloring of stainless steel alloys. The woes that this step gave me, I can not believe the armed resistance stainless puts up against developing any colored oxide layer under any circumstance. I guess it is not called "stainless" in vain.
The commercial processes for this purpose mostly utilize the action of chromic acid, hence hexavalent chromium under high temperature and electrochemical action....an utterly nasty approach that I do not want to have any intimate contact with. Browsing through patents several alternate chromium free approaches were suggested: dilute phosphoric acid solutions at elevated temperatures, caustic permanganate solutions, acidic permanganate solutions, caustic electrolytic treatments, etc....most of which simply do not work, create a layer that washes off or require a very fine tuning of parameters. The only chemical chromium free concoction that gave any effect of developing a somewhat colored layer on stainless was 70% sulfuric acid and potassium permanganate mixture on prolonged contact. A 316 grade stainless strip developed a faint golden/brown interference layer after being left to soak in this solution over night.
I was about to give up, as I stumbled upon the approach of coloring stainless alloys via reversed pulsed electrolysis in ammonium molybdate solutions. I'm sorry, but for the life of me I can not find the patent reference at the moment....
To test it out I prototyped a mosfet H-bridge driven by 2 IR2110 chips and a rectangular pulse generator.

DSCF1549.JPG - 440kB
Fig. 7 The H-bridge for pulsed electrolysis (anodic/cathodic duty and frequency adjustable)


DSCF1530.JPG - 363kB
Fig. 8 A little stand for supporting the electrolysis cell and electrodes (one might recognize the oxide coated details from previous steps in the construction)


DSCF1539.JPG - 299kB
Fig.9 The system operating from a 4V Li cell with a 30g/l ammonium heptamolybdate water solution in the beaker and both electrodes from stainless steel 316 and 304.


DSCF1544.JPG - 274kB
Fig.10 Amazing interference layer formed on a regular stainless steel spoon with 50% duty cycle for anodic period (hence cathodic too) in the ammonium molybdate solution after 4min at room temperature and 5Hz frequency




Exact science is a figment of imagination.......
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 28-2-2018 at 14:47


Now that is Superb !

The black effect with just pot perchlorate and ammonium nitrate is awesome.

The coloring of the stainless spoon with AC is reminiscent of heating it to a very high temperature.




View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 28-2-2018 at 15:01


Quote: Originally posted by aga  
Now that is Superb !

The black effect with just pot perchlorate and ammonium nitrate is awesome.

The coloring of the stainless spoon with AC is reminiscent of heating it to a very high temperature.


Yes...from the pictures it looks kind of like a layer that is formed during TIG welding, but in first person the effect is amazingly different. The colour changes from a golden hue through red and into the electric iridescent blue depending on the angle that it is viewed from....quite amazing effect. Also the colour is dependant on the residence time and current density in cell and changes from purple blue to a deep golden greenish tint with increasing reaction time. Also if one dips the spoon into water, the colour vanishes completely and only a clean stainless silver surface is seen....after drying the colours reemerge. A purely wave interference related phenomenon... :)

DSCF1545.JPG - 339kB


Same spoon full of water :



DSCF1565.JPG - 285kB


Water dumped out:



DSCF1567.JPG - 243kB

[Edited on 28-2-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1685
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 28-2-2018 at 15:14


I think the smoother the surface the better the colors, at least it was for some titanium tubing that was sanded as smooth as possible on my lathe. But I just used a propane torch and you'd have to coat these tubes with a clear epoxy or something to hopefully keep the colors from wearing off or degrading. I press fit an alligator clip in the end of one smaller tube and it was kind of a cute thingamajig of some sort.
http://www.pulse-jets.com/phpbb3/download/file.php?id=13570&...
http://www.pulse-jets.com/phpbb3/download/file.php?id=13569&...
http://www.pulse-jets.com/phpbb3/download/file.php?id=13572&...

May I ask where you got that aluminum bottle next to the rum or what was in it?
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 28-2-2018 at 15:23


Quote: Originally posted by Morgan  
I think the smoother the surface the better the colors, at least it was for some titanium tubing that was sanded as smooth as possible on my lathe. But I just used a propane torch and you'd have to coat these tubes with a clear epoxy or something to hopefully keep the colors from wearing off or degrading. I press fit an alligator clip in the end of one smaller tube and it was kind of a cute thingamajig of some sort.

May I ask where you got that aluminum bottle next to the rum or what was in it?


Definately the surface finish is most important.....the oxide layers are so thin that they do not hide anything and all of the defects or structures shine through the coating. The spoon was sanded with a 2000grit wet abrasive paper before electrolysis...

Sorry to dissapoint you, but that bottle is actuallly PE and holds a special e-cigarette liquid....if you look closely you can see the liquid level faintly shinig through the bottle wall :) And the rum bottle holds a homemade superior "grand marnier" liquor, albeit it do does look very much like the original beverage that was once contained in it....apperances are deceiving

[Edited on 28-2-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1685
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 28-2-2018 at 17:20


Ah yes, I see the liquid level. Seems so obvious now. I like those mild steel doodads you made for the lab stand.
I used 2000 grit paper too for the titanium tubing. A smooth surface brought out a glossiness to the titanium as well as more varied colors. If I didn't polish the tubing very well only blues and browns would form.
http://www.pulse-jets.com/phpbb3/download/file.php?id=13562&...

One time I thought it would be fun to use my 6 foot length of titanium tubing to make a multi-colored banded pole and clear coat it to try to keep the exotic colors. I think these colors were formed when I sanded the tubing somewhat but not as pretty or varied as if I got the surface really smooth before heating it.
http://www.pulse-jets.com/phpbb3/download/file.php?id=13564&...

[Edited on 1-3-2018 by Morgan]
View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 747
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 1-3-2018 at 11:35


Niobium is very colourful and easy to get to work if you can obtain some
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 1-3-2018 at 12:57


Quote: Originally posted by yobbo II  
Niobium is very colourful and easy to get to work if you can obtain some


True....and it is not a problem to obtain some niobium, but easy things are boring :) I specifically wanted to get coloration on stainless steel....I find it fascinating for some reason. I guess partly because I like machining different equipment from stainless and would like to add some color accents to it.
Imagine a fractionating column polished to a mirror sheen and coated in such an interference layer....now that would be awesome :D !




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 6-3-2018 at 10:54


Some nice color development with 50% anodic duty at 10Hz on 316 stainless (duration of treatment not registered precicely, but about 60min):

DSCF1572.JPG - 735kB



Another sample of unknown high nickel stainless (it was a real pain to machine, hence the presumption of high Ni content). Same conditions of treatment (except lower current density due to bigger detail), duration 20min:

DSCF1573.JPG - 811kB


The camera distorts the coloration a bit, but the round disc developed a really beautiful irradiating lilac around outer edges :)









Exact science is a figment of imagination.......
View user's profile View All Posts By User
Akhil jain
Hazard to Self
**




Posts: 83
Registered: 19-2-2018
Member Is Offline

Mood: No Mood

[*] posted on 6-3-2018 at 12:22


I think that black color could be due to the carbon content in stainless steel . And those colors I think is due to oxides of Cr and Fe
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 15-3-2018 at 11:54


Well....now that is a strange one for sure:

DSCF1597.JPG - 839kB

This is definately not chromium oxide layer, but should presumably be a very thin layer of lead dioxide. The layer was decently attached, but could be partly rubbed off with enough vigor (on the tip of the metal strip).
This particular specimen resulted from a clumsy attempt at trying to electrodeposit lead dioxide onto a stainless steel strip from a solution of lead acetate, acetic acid and ammonium nitrate.
Instead of forming a brown or black deposit I got this rainbow effect....it is not iridecent the way the other samples formed in the molybdate AC bath, but looks rather like a colored tarnish.
Very interesting....




Exact science is a figment of imagination.......
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 15-3-2018 at 12:16


That one certainly looks pretty.

The vivid colours come out better in the photo than the iridescent ones.




View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 15-3-2018 at 12:40


Quote: Originally posted by aga  
That one certainly looks pretty.

The vivid colours come out better in the photo than the iridescent ones.


It is a quite profoundly colorful coincidence for sure :D
Considering that the result should have looked black to deep drown if it really was lead dioxide, makes it even stranger.

What I actually did was to elecrolytically dissolve lead electrodes in ammonium nitrate solution using AC electrolysis and precipitated lead hydroxides as a result. I then acidified the solution with acetic acid to dissolve the precipitate and bring the lead into solution. I then proceeded to DC electrolysis with the abovementioned stainless strip as the anode in an attempt to partially electrodeposit the soluble lead as the dioxide on the stainless. That resulted in this colorful monstrocity.
I must admit that the coating began as a promising brown translucent layer and then evolved into different colored areas.
Quite an unexpected result...

[Edited on 15-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
mayko
International Hazard
*****




Posts: 1218
Registered: 17-1-2013
Location: Carrboro, NC
Member Is Offline

Mood: anomalous (Euclid class)

[*] posted on 29-3-2018 at 16:09


How sensitive is the effect to the specifics of the power supply (current, voltage, duty cycle)? Does it work with steady current, or is pulsed electrolysis strictly necessary?



al-khemie is not a terrorist organization
"Chemicals, chemicals... I need chemicals!" - George Hayduke
"Wubbalubba dub-dub!" - Rick Sanchez
View user's profile Visit user's homepage View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 3-5-2018 at 03:56


Quote: Originally posted by mayko  
How sensitive is the effect to the specifics of the power supply (current, voltage, duty cycle)? Does it work with steady current, or is pulsed electrolysis strictly necessary?


The rate of thickening of the oxide coating is dependant on current density and higher currents tend to bring about the coloration change during a shorter period of time.
I have not tried this bath in DC current mode, so I can not comment on wether it works, but I would assume that at least some coloration change can be observed on either of the electrodes.
E.g. I observed a rainbow style coloration change on a stainless spoon that was used as a cathode in dilute phosporic acid solution in DC mode. The coating was very thin and fragile and could be wiped off quite easily.




Exact science is a figment of imagination.......
View user's profile View All Posts By User
rolynd
Harmless
*




Posts: 16
Registered: 13-12-2004
Location: At Home
Member Is Offline

Mood: No Mood

[*] posted on 29-5-2018 at 00:24


Pulse/pulse reverse electrolysis is interesting. I have been using that with copper plating/electroforming to get dense and ductile deposits with good results. I have used a commercial H-bridge controlled by an arduino. but "on the fly" adjustment of freq/duty cycle is not possible with that so easily. A simple frequency generator does not hook up to those because they require multiple inputs(enable,fwd,rev) whereas a freq generator does put out only a pwm signal. Do you have a schematic/ parts list for your h-bridge design that you are willing to share?
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 29-5-2018 at 11:54


Quote: Originally posted by rolynd  
Do you have a schematic/ parts list for your h-bridge design that you are willing to share?


Sure...I just need to find the time to draw it up correctly. A word of caution regarding this schematic though: I'm not sure about the ruggedness of the dead time management of this setup for cross conduction prevention. So there should be a suitable current limiting resistor present before the h-bridge to keep the mosfets from shorting out in case of cross conduction taking place during switching (or one cold use a high impedance power supply that can not sink huge amounts of amperes).

You can reference this design....it is pretty much the same setup that I use:

http://microcontrollerslab.com/wp-content/uploads/2014/08/ci...

The mosfets can be chosen liberally from a wide range of available parameters, but for electrolysis anything that handles the required currents and is rated upward of 20V can be used in principle. I used IRF3205 in my setup because they were at hand and cheap as dirt. As long as you do not switch inductive loads, like motors or transformers, there should be no problems regarding inductive kickback that can ruin a schematic in a hurry and be quite complicated to snub correctly.


[Edited on 29-5-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
rolynd
Harmless
*




Posts: 16
Registered: 13-12-2004
Location: At Home
Member Is Offline

Mood: No Mood

[*] posted on 29-5-2018 at 19:11


thanks , a schematic would be splendid. I am not an electronics whiz unfortunately. I am better at chemistry... the part I am having trouble with is how to hook up the pwm generator to such a circuit. as far as I understand it the IR2110 drivers each have two signal inputs (A,B)/(C,D) for the high and low side mosfets. While AD and and BC are made common to turn on/off the respective Q1Q4 or Q2Q3 mosfets that still leaves me with 2 signal inputs to make the bridge go fwd/rev - the pwm signal generator only puts out one signal though? When using an arduino as a signal source I just designate 2 pins to that task - but every time I want to change freq or duty cycle I have to modify the sketch and reupload it. would be much more convenient if I could use one of these adjustable signal generators to provide the input. thats the part that has me sitting, scratching my head?
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 29-5-2018 at 23:31


Quote: Originally posted by rolynd  
thanks , a schematic would be splendid. I am not an electronics whiz unfortunately. I am better at chemistry... the part I am having trouble with is how to hook up the pwm generator to such a circuit. as far as I understand it the IR2110 drivers each have two signal inputs (A,B)/(C,D) for the high and low side mosfets. While AD and and BC are made common to turn on/off the respective Q1Q4 or Q2Q3 mosfets that still leaves me with 2 signal inputs to make the bridge go fwd/rev - the pwm signal generator only puts out one signal though? When using an arduino as a signal source I just designate 2 pins to that task - but every time I want to change freq or duty cycle I have to modify the sketch and reupload it. would be much more convenient if I could use one of these adjustable signal generators to provide the input. thats the part that has me sitting, scratching my head?


The signal generator I use actually has two outputs that run in reverse phase. Inputs on the IR2110s are bridged in such a way that the high signal triggers one upper mosfet and one lower mosfet at the opposing side of H-bridge. Thus allowing to drive current in one or the other direction depending on which signal generator output is active. I have no idea about the dead time between the switching of the signal generator outputs though....for worst case scenario I suspect there is none. You can also realize this schematic with only a single output signal generator, but you have to include a signal reverse stage as the second input for the IR2110 stages. It can be done with a transistor and a suitable resistor.




Exact science is a figment of imagination.......
View user's profile View All Posts By User
rolynd
Harmless
*




Posts: 16
Registered: 13-12-2004
Location: At Home
Member Is Offline

Mood: No Mood

[*] posted on 30-5-2018 at 04:02



Quote:

You can also realize this schematic with only a single output signal generator, but you have to include a signal reverse stage as the second input for the IR2110 stages. It can be done with a transistor and a suitable resistor.


Common emitter?

if you have a part number or link to the pulse generator that would also be nice - the ones i have seen with double output are in sync.

pulse generator

.
View user's profile View All Posts By User
mayko
International Hazard
*****




Posts: 1218
Registered: 17-1-2013
Location: Carrboro, NC
Member Is Offline

Mood: anomalous (Euclid class)

[*] posted on 25-1-2019 at 15:52


I've tried the black oxide bath a few times now and I haven't gotten it to work :( I've been using stainless steel utensils and strips cut out of a steel tray, scrubbed w/fine stainless steel and washed with detergent & water.

the first time I messed up trying a 1/10 scale experiment, forgetting to scale the chlorate and mixing a solution of:
1.00 g NH4NO3
0.15 g KClO3
100mL H2O

The referenced patent says that "Including too much chlorate will result in a blue cast of the coating or in coatings which are powdery and there fore undesirable", but after 30 minutes of boiling in this bath, the steel pieces appeared unchanged

Next, I prepared a proper batch in a 1L volumetric flask, consisting of:
10.03 g NH4NO3
0.150 g KClO3 (freshly recrystalized).

However, this also had no impact on the steel pieces after 30+ minutes at boiling. The patent suggested that acidic conditions are helpful, so I added 2 drops conc. H2SO4 to ~150 mL bath but this also didn't work.

Is there something I'm missing? :o :(





al-khemie is not a terrorist organization
"Chemicals, chemicals... I need chemicals!" - George Hayduke
"Wubbalubba dub-dub!" - Rick Sanchez
View user's profile Visit user's homepage View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 28-1-2019 at 01:36


Quote: Originally posted by mayko  
I've tried the black oxide bath a few times now and I haven't gotten it to work :( I've been using stainless steel utensils and strips cut out of a steel tray, scrubbed w/fine stainless steel and washed with detergent & water.

the first time I messed up trying a 1/10 scale experiment, forgetting to scale the chlorate and mixing a solution of:
1.00 g NH4NO3
0.15 g KClO3
100mL H2O

The referenced patent says that "Including too much chlorate will result in a blue cast of the coating or in coatings which are powdery and there fore undesirable", but after 30 minutes of boiling in this bath, the steel pieces appeared unchanged

Next, I prepared a proper batch in a 1L volumetric flask, consisting of:
10.03 g NH4NO3
0.150 g KClO3 (freshly recrystalized).

However, this also had no impact on the steel pieces after 30+ minutes at boiling. The patent suggested that acidic conditions are helpful, so I added 2 drops conc. H2SO4 to ~150 mL bath but this also didn't work.

Is there something I'm missing? :o :(



What is the source of your ammonium nitrate? If you used contemporary fertilizer grade, then note that these are usually AN mixes with ammonium sulfate to render them undetonable. The sulfate content will hinder the operation of the bath, although I've found these mixes to work on simple high carbon steels. On alloy steels they do not tend to develop proper coating. So make sure you have pure AN, not a mixture.
Did you by chance immerse the parts in cold solution and then begin to heat it up with the parts in it? It is preferable to immerse the parts into preheated bath. I've always done it this way. I'm not sure if the heating up with the parts in the bath has a detrimental effect on the process, but it might. I've not exactly tried it out this way.
Have you tried all of your experiments with the steel strips from the same source (the steel tray)? If so then try other pieces from various sources. Something simple like nails, bolts, old drill bits. Be sure the steel object receiveing the blackening treatment is not a stainless alloy...the bath only works on ferrous alloys that are able to rust. The black oxide is a form of rust, just a very dense and decorative one.
Sometimes one finds a steel alloy that just does not want to develop black oxide in this bath. I've come across several alloys that by the look and properties are mild steel, but resist developing any black in the nitrate bath. Perhaps you suffered the same fate? Also make sure the steel bits are not galvanised or surface treated with some kind of a coating....zinc contaminates the bath and it will not work. Also phosphates are to be avoided in this bath.
Did you notice the solution in the bath turning rusty when you boiled the parts? If the bath is working properly there should be a rusty brown precipitate (sometimes even black) forming in the solution some minutes after immersing the parts. If the solution stays totally clear then the alloy that you used is not reacting with the bath constituents and does not form any oxide.
And by all means you can omit the chlorate additive, it is not imperitive for the operation of the bath at all. Just ammonium nitrate solution shall work very well and probably create less trouble. Also the concentration of ammonium nitrate seems to be not critical and it will work in a wide range. I've sometimes boiled off half of the water from the bath without any detrimental effects to the coating.
Also you do not need to dispose of the bath solution after use....just let it cool down and store it in a plastic container. You can use the same solution basically indefinitely. I've been using the same batch for several years and for the coating of dozens of parts. Still works like on the very first use.

I've also noticed that the bath needs access to atmospheric oxygen to develop the coating. If the vessel is closed or there are many parts loaded into the bath, then a defficiency in oxygen is the result and a slow coating process can follow. Also this can be seen from the fact that sharp inner corners, orifices, recesses and internal surfaces of parts tend to coat slower than exposed surfaces....there is restricted circulation and oxygen transport to these areas. It actually helps sometimes to lift the part out of the hot solution and let it dry above the bath for a few seconds without flushing off the bath solution....this will usually trigger the oxide formation if it should not start normally or in areas that are hard to reach.

Hope this is of some help :)

[Edited on 28-1-2019 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 30-1-2019 at 11:25


Been doing some more experimentation on improving the AC electrolysis coloration effect on stainless alloys.
Have found out that the AC coloration effect actually works to some degree with a great number of rather common salts. The frequency for efficient color development seems to reside within the approximate range of 2-10Hz.


Golden orange coloration developed on stainless spoon in magnesium nitrate solution (30g/l 5Hz):
DSCF1826.JPG - 1.1MB DSCF1825.JPG - 1MB


Subtle golden coloration formed on stainless spoon in sodium perchlorate solution (10g/l 5Hz):

DSCF1829.JPG - 1.2MB DSCF1828.JPG - 1.1MB


Some different colored examples from various electrolytes:

DSCF1836.JPG - 1.1MB


Very intense polychromic effect from ammonium molbdate/ manganese sulfate electrolyte (30g/l amm. molybdate 1,2g/l manganese sulfate 5Hz) :

DSCF1884.JPG - 1.2MB DSCF1885.JPG - 1.1MB DSCF1891.JPG - 1.1MB

Even sodium bicarbonate solution develops a faint golden hue on 316 stainless, but very slowly...




Exact science is a figment of imagination.......
View user's profile View All Posts By User
andy1988
Hazard to Others
***




Posts: 135
Registered: 11-2-2018
Location: NW Americus ([i]in re[/i] Amerigo Vespucci)
Member Is Offline

Mood: No Mood

[*] posted on 31-1-2019 at 05:55


The black oxide bath looks very useful, thank you.

Great read here I thought I'd share:
Quote:
Magnetite (or Fe3O4) is an elaborate kind of rust - a regular lattice of oxygen and iron atoms. But this material plays an increasingly important role as a catalyst, in electronic devices and in medical applications.

Scientists at the Vienna University of Technology have now shown that the atomic structure of the magnetite surface, which everybody had assumed to be well-established, has in fact been wrong all along. The properties of magnetite are governed by missing iron atoms in the sub-surface layer. "It turns out that the surface of Fe3O4 is not Fe3O4 at all, but rather Fe11O16", says Professor Ulrike Diebold, head of the metal-oxide-research group at TU Wien (Vienna). The new findings have now been published in the journal Science.

Perhaps the most surprising property of the magnetite surface is that single atoms placed on the surface, for instance gold or palladium, stay perfectly in place instead of balling up and forming a nanoparticle. This effect makes the surface an extremely efficient catalyst for chemical reactions - but nobody had ever been able to tell why magnetite behaves that way.

Very often, the properties of metal oxides depend on oxygen vacancies in the topmost atomic layers. Depending on the environment, some oxygen atoms on the surface may be missing. This can dramatically influence the electronic properties of the material. "Everyone in our community thinks about missing oxygen atoms. That is why it took us quite a while to figure out that it is in fact missing iron atoms that do the trick", says Gareth Parkinson. [1]




View user's profile View All Posts By User
mayko
International Hazard
*****




Posts: 1218
Registered: 17-1-2013
Location: Carrboro, NC
Member Is Offline

Mood: anomalous (Euclid class)

[*] posted on 31-1-2019 at 20:45


I got the black oxide bath to work. I didn't catch that it didn't work on stainless, but it definitely worked on magnetic coathanger wire. The only problem I had was the solution boiling off! I guess I could use a reflux setup of some sort.

I've got a PWM and some H-bridges on the way :)




al-khemie is not a terrorist organization
"Chemicals, chemicals... I need chemicals!" - George Hayduke
"Wubbalubba dub-dub!" - Rick Sanchez
View user's profile Visit user's homepage View All Posts By User