Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
 Pages:  1  
Author: Subject: US Pyrex kitchenware not Borosillicate glass!
RogueRose
International Hazard
*****




Posts: 1597
Registered: 16-6-2014
Member Is Offline


[*] posted on 5-2-2017 at 05:43
US Pyrex kitchenware not Borosillicate glass!


Had some Pyrex break and the way it shattered made me question the material but never looked into it until now. It looks like the type of glass is dependent upon region. Not too good IMO.


The following can be found on this page: https://en.wikipedia.org/wiki/Borosilicate_glass
Quote:

The European manufacturer of Pyrex, Arc International, uses borosilicate glass in its Pyrex glass kitchen products;[1] however, the U.S. manufacturer of Pyrex kitchenware uses tempered soda-lime glass.[2] Thus Pyrex can refer to either soda-lime glass or borosilicate glass when discussing kitchen glassware, while Pyrex, Bomex, Duran, TGI and Simax all refer to borosilicate glass when discussing laboratory glassware. The real difference is the trademark and the company that owns the Pyrex name. The original Corning ware made of borosilicate glass was trademarked in capital letters (PYREX). When the kitchenware division was sold, the trademark was changed to lowercase (pyrex) and switched to low thermal-expansion soda-lime glass.

View user's profile View All Posts By User
Geocachmaster
Hazard to Others
***




Posts: 146
Registered: 5-3-2016
Location: Maine, USA
Member Is Offline

Mood: Corroded, just like my spatulas

[*] posted on 5-2-2017 at 06:07


Yes, I think it has not been borosilicate for quite some time now. Over in Europe Pyrex brand kitchenware is still boro glass IIRC (edit: I see that's in the quote now). Kitchen glassware in general has rather thick glass, which is undesirable because it increases the chance of cracking while heating, even if it does increase durability.

[Edited on 2/5/2017 by Geocachmaster]
View user's profile View All Posts By User
vmelkon
National Hazard
****




Posts: 669
Registered: 25-11-2011
Location: Canada
Member Is Offline

Mood: autoerotic asphyxiation

[*] posted on 5-2-2017 at 06:26


Yes, we know.

The part that I didn't know was that Corning sold off their kitchenware division. Man, these guys sell everything.
In india, they established a chemistry glassware company and then sold it off. It is now under the name of Bomex.




Signature ==== Is this my youtube page? https://www.youtube.com/watch?v=tA5PYtul5aU
We must attach the electrodes of knowledge to the nipples of ignorance and give a few good jolts.
Yes my evolutionary friends. We are all homos here.
View user's profile View All Posts By User
RogueRose
International Hazard
*****




Posts: 1597
Registered: 16-6-2014
Member Is Offline


[*] posted on 5-2-2017 at 06:33


Well I'm glad that other know, whether some or most, IDK, but it does seem a little odd that it differs from the US to EU, especially if someone reads that Pyrex is Boro somewhere but doesn't mention that it can vary with intended use and region of distribution.
View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*****




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 7-2-2017 at 00:41


Yeah, those bastards took advantage of the fact that "Pyrex" is their trademark and not actually synonymous with "borosilicate glass". So they can label anything they want to as "Pyrex" and there's nothing we can do about it, except learn to recognize borosilicate glass when we see it. (hint: if it's thick and has a green tint, don't use it for chemistry!)

edit: I wonder if there's grounds for a class-action lawsuit, alleging that they knowingly misled people by doing this? LOTS of people, even non-chemists have had glass cookware explode on them because they thought that "Pyrex" meant "borosilicate".

[Edited on 2/7/17 by Melgar]
View user's profile View All Posts By User
Praxichys
International Hazard
*****




Posts: 1063
Registered: 31-7-2013
Location: Detroit, Michigan, USA
Member Is Offline

Mood: Coprecipitated

[*] posted on 7-2-2017 at 09:55


I have a large collection of Pyrex pans and dishes that I use for chem all the time. Just because you can't heat it directly doesn't make them less useful.

I use the large Pyrex mixing bowls as ice baths or warm water baths with an immersion heater. I fill one with xylenes to soak other glassware in for removing sulfur, since xylenes don't play nice with plastics. They're great for crashing large, acidic solutions into cold water (like nitrations) and you can get a 2-liter bowl at the goodwill store for $3, as opposed to a 2-liter boro beaker which is like $30.

Pyrex pans and baking dishes can be safely heated over a steam bath and in the oven, so they make great surfaces for drying wet crystals, evaporating solutions, and regenerating desiccants. I do it all the time in my videos.

[Edited on 7-2-2017 by Praxichys]




View user's profile Visit user's homepage View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 7-2-2017 at 10:08


Why, exactly, is Kitchen-ware being discussed on a Chemistry forum ?

Oh ! I see. If it's not politics any other garbage is fine ? OK.

Personally i like the french steel-teflon flan trays with detachable bottom plate for making small quiches. Perfect pro-looking result and instant quiche-release.

Recently i got one with perforations, giving a really crispy texture to the pastry.




View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*****




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 7-2-2017 at 10:14


Quote: Originally posted by Praxichys  
I have a large collection of Pyrex pans and dishes that I use for chem all the time. Just because you can't heat it directly doesn't make them less useful.

I think what gets most people is the fact that you also can't cool it directly. Like, they'll set a hot Pyrex™ pan on a cold stovetop and have it explode. And I agree that having semi-heat-resistant glass bowls and such is useful, it's just a bit disingenuous for them to allow it to be labeled using a brand name that has become shorthand for "borosilicate glass". (Incidentally, since we use "pyrex" all the time here to mean that, I guess we should capitalize it for the brand, and use lowercase to mean borosilicate? We need conventions!)

It'd be like having Kleenex-brand burlap, or Band-aid brand nicotine patches. Not useless so much as inconsiderate.

aga: Because a lot of people use glass cookware for chemistry. I used to have a Pyrex™ measuring cup that was graduated in mL and ounces, until it exploded on me when heating it. Until then, I too, thought "Pyrex" meant borosilicate.

[Edited on 2/7/17 by Melgar]
View user's profile View All Posts By User
battoussai114
Hazard to Others
***




Posts: 235
Registered: 18-2-2015
Member Is Offline

Mood: Not bad.... Not bad.

[*] posted on 7-2-2017 at 10:35


Doesn't soda lime glass also have a higher percentage of soluble glass besides not being resistant to thermal shock? While it's probably not a major problem for non-analytic work, it's worth keeping in mind.



Batoussai.
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 7-2-2017 at 11:26


Quote: Originally posted by Melgar  
... I too, thought "Pyrex" meant borosilicate.

I also use whatever i have that is suitable at the time.

Currently i got about quarter a kilo of sodium sulplate drying on the lid of a 20L paint bucket.

"Pyrex" has always just been a brand name, synonymous with kitchen glass that can go in an oven.

What it is composed of is pretty much irrelevant - it's not sold as chemistry apparati (which also shatter if treated badly).

My point is : why is so much said about trivial non-Chemistry nonsense these days ?

Someone does a Grignard and gets 3 or 4 replies.

Mention some kitchenware breaking and get how many ? Sheesh !




View user's profile View All Posts By User
Melgar
Anti-Spam Agent
*****




Posts: 2004
Registered: 23-2-2010
Location: Connecticut
Member Is Offline

Mood: Estrified

[*] posted on 7-2-2017 at 12:30


Quote: Originally posted by aga  
Someone does a Grignard and gets 3 or 4 replies.

Mention some kitchenware breaking and get how many ? Sheesh !

If you're trying to say something, this is a really weird battle to pick, considering improvised glassware is very much on-topic in this forum. Pyrex brand kitchenware used to always be made out of borosilicate glass, and still is in many countries. Being able to discern the difference between Pyrex-brand borosilicate cookware and Pyrex-brand tempered soda-lime cookware is fairly important if we need real borosilicate glass, improvised or not, for a particular reaction or purpose.
View user's profile View All Posts By User
S.C. Wack
bibliomaster
*****




Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline

Mood: Enhanced

[*] posted on 7-2-2017 at 15:16


http://www.sciencemadness.org/talk/viewthread.php?tid=3384
http://www.sciencemadness.org/talk/viewthread.php?tid=12170




"You're going to be all right, kid...Everything's under control." Yossarian, to Snowden
View user's profile Visit user's homepage View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 7-2-2017 at 15:33


The glassware used is definitely on-topic.

ONLY of the glassware is ever used.
(corningware is also good)

No evidence of any chemistry At All yet from the OP, so i dunno.




View user's profile View All Posts By User
zwt
Hazard to Self
**




Posts: 84
Registered: 1-8-2016
Member Is Offline

Mood: No Mood

[*] posted on 7-2-2017 at 16:06


Quote: Originally posted by aga  
No evidence of any chemistry At All yet from the OP, so i dunno.
Here's some:
http://www.sciencemadness.org/talk/viewthread.php?tid=26378&...
http://www.sciencemadness.org/talk/viewthread.php?tid=61783&...
http://www.sciencemadness.org/talk/viewthread.php?tid=70072#...
Looks like attempts to prepare and purify reagents, the necessary first steps for those who can't just buy everything they need. You shouldn't have a problem with that - you've also been complaining recently about people who don't prepare their own reagents.
View user's profile View All Posts By User
Amos
International Hazard
*****




Posts: 1406
Registered: 25-3-2014
Location: Yes
Member Is Offline

Mood: No

[*] posted on 7-2-2017 at 16:57


Quote: Originally posted by aga  
The glassware used is definitely on-topic.

ONLY of the glassware is ever used.
(corningware is also good)

No evidence of any chemistry At All yet from the OP, so i dunno.


boi how many of your posts even contain chemistry? Over 6000 comments and probably somewhere just under 1% provide evidence that you've done any.
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6367
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 7-2-2017 at 18:54


Quote: Originally posted by Amos  

how many of your posts even contain chemistry? Over 6000 comments and probably somewhere just under 1% provide evidence that you've done any.

That is probably a reasonable question to aga but it is not a conversation that I think needs to happen in public. And the same goes for aga's questioning of the chem content of other users' posts.

We all know that getting some good experimental chemistry in and sharing the results is the most satisfying thing about this board. But there are many reasons why it does not always happen. Life has a way of getting in the way for all of us. I come here to think chem, read chem and discuss chem even when I cannot do chem. I think that is ok.


Back on topic, I do have among my lab equipment a range of repurposed kitchenware items. I started collecting those before I got into buying proper glassware. Although they are often useful and frequently cheaper, I do not trust the glass items to resist any kind of thermal shock or high temperatures. Maybe I am being overly cautious. But I have seen exploding kitchenware before and it just aint pretty.
View user's profile View All Posts By User
Amos
International Hazard
*****




Posts: 1406
Registered: 25-3-2014
Location: Yes
Member Is Offline

Mood: No

[*] posted on 7-2-2017 at 22:00


Agreed but I have my limits.

The only piece of kitchenware I stock at the moment is a big casserole dish I use for crystallization, which often entails pouring a liter of boiling liquid directly into it. I often put it directly on a hot plate to evaporate solutions, too, just being careful to keep the temperature low and ramp it up slowly. Hasn't caused any problems in about 2 years, so it can't all be that awful.
View user's profile View All Posts By User
JJay
International Hazard
*****




Posts: 3440
Registered: 15-10-2015
Member Is Offline


[*] posted on 7-2-2017 at 22:36


I've use soda lime cookingware for a few lab tasks, generally trying to limit its exposure to temperature extremes that it would encounter in normal use, and I haven't run into any problems. That stated, I wouldn't try heating it with a blowtorch or putting it over a Bunsen burner.



View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3775
Registered: 8-2-2015
Member Is Offline


[*] posted on 8-2-2017 at 02:31


worth remembering ... Otto Schott started selling DURAN borosilicate glass in 1893,
anything before that was soda-lime glass ...
i.e. Alchemy, the chemistry renaisance and all pre-20th century chemistry :D

My borosilicate glassware with ground glass joints would have given Alchemists wet dreams :P

https://en.wikipedia.org/wiki/Borosilicate_glass






CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
RogueRose
International Hazard
*****




Posts: 1597
Registered: 16-6-2014
Member Is Offline


[*] posted on 9-2-2017 at 17:14


Just out of curiosity, I'm wondering about coffee pots like the ones for coffee machines. I've seen a lot of people use them on a burner (usually gradually heating) as well as over a mild flame like an alcohol lamp. The glass is very thin compared to the Pyrex measuring cups and other Pyrex "cookware" like small 1c storage dishes (great for evap containers for non-corrosive materials).

The glass on these coffee pots is very similar in thickness and color/transparency to the Pyrex beakers I have as well as Pyrex flasks, test tubes, petri dishes, etc. They also break similarly as well with being dropped or hit with something heavy.

I can't imagine these are soda-lime but more like some boro type. I did heat NaHCO3 to not temp (350F -400) and them placed on a cold metal stove to see if it could crack and it seemed fine. It was an older Mr Coffee purchased at a thrift shop in the US. I can't speak to other pots that may seem similar but of "cheaper" brand or possibly construction.


Oh and for note, the REASON I brought this topic up is I had read in a post, on this board, that all pyrex was borosilicate and was indeed something to look for - which is why they went to rubbage/garage sales and thrift at times because they found great uses for these when doing various non-crucial experiments. Well I had an explosion experience with one and months later I posted this thread when I found the infor I linked to above.

AS always, some member (Cartman in his elder years - Respect my authoritah!!! and Homer Simpson hybrid) feels the need to make accusations and talk smack when there may be many other people who saw the name post I did and could get hurt by this. Then it lead to personal attacks whe all he had to do was a search, but his type just spews insults to anyone who Dares to not act in accordance to how HE/THEY believe is the proper and only way.

I thank all those who have mentioned something on my behalf and realize the glaring contradiction of 2 people, joined a couple months apart, one with 30x my posts (and a much MUCH higher non-chemistry post count than ANYONE on this forum) with a percent of member belligerence that is matched by NO ONE else on the board - chasing newbies away for many unfounded reasons. This is what almost ANY mod and member would call a troll.

Again, I thank those who recognize that not all member have access to the means to perform complex reactions that require distillation kits or vacuum filtration but by asking questions, especially those designed to highlight potential danger issues, is a magnitude more helpful that negativity spewed by some.



[Edited on 10-2-2017 by RogueRose]
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1725
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 10-2-2017 at 06:03


There's this stuff.
https://www.youtube.com/watch?v=rc6EH2Gb90o
http://www.kavalier.cz/en/section/15-general-information.htm...
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3775
Registered: 8-2-2015
Member Is Offline


[*] posted on 10-2-2017 at 07:18


Some cafetieres have nice 'beakers' at their core,
I broke a 2l one and I have a 600ml and an 800ml one, from charuty shops.
Some are PYREX, some are toughened glass, all can handle boiling water.




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
Morgan
International Hazard
*****




Posts: 1725
Registered: 28-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 9-9-2017 at 14:55


My sister sent me a couple of these bottles out of the blue having mentioned I liked some thin-walled borosilicate food storage containers that looked something like large petri dishes with high sides and lids. Happy little bottles I guess ...
http://1.bp.blogspot.com/-7IKum7Vkdoo/UYotsjH-b5I/AAAAAAAAAF...
https://static.fpv24.com/img/product/re/retblrp11gl47ly28/so...
http://www.retap.com/products/
http://www.retap.com/en/wp-content/uploads/2014/10/table-wit...
https://cdn4.thegrommet.com/media/catalog/product/cache/1/im...
https://cdn3.volusion.com/devfd.zdvnj/v/vspfiles/photos/rt1-...
DSC_0068.JPG - 150kB DSC_0066.JPG - 146kB DSC_0065.JPG - 115kB

[Edited on 9-9-2017 by Morgan]
View user's profile View All Posts By User
SWIM
National Hazard
****




Posts: 970
Registered: 3-9-2017
Member Is Offline


[*] posted on 9-9-2017 at 16:55


Quote: Originally posted by aga  


Personally i like the french steel-teflon flan trays with detachable bottom plate for making small quiches. Perfect pro-looking result and instant quiche-release.

Recently i got one with perforations, giving a really crispy texture to the pastry.


A flan tray with perforations? Doesn't it leak badly when you melt the sugar?
I use ceramic ramekins mostly, sometimes a PYREX baking dish, but never a pyrex baking dish.
View user's profile View All Posts By User
Dr.Bob
International Hazard
*****




Posts: 2806
Registered: 26-1-2011
Location: USA - NC
Member Is Offline

Mood: Mildly disgruntled scientist

[*] posted on 10-9-2017 at 14:44


Sadly, much cookware in the US has been soda lime for years now. The index of refraction is different, but hard to measure trivially, and there are several times of soda lime glass, so not trivial to tell them apart without a little work. But there are useful properties of both. The main issue is that making borosilicate glass pollutes more than soda lime, thus making it in the US is nearly impossible now, just like doing any chemistry is tough and expensive now.
View user's profile View All Posts By User
 Pages:  1  

  Go To Top