Author: Subject: lead into water - fine, pewter, not so
Scalebar
Hazard to Self
**




Posts: 54
Registered: 6-5-2016
Location: Europe!
Member Is Offline

Mood: Looking for a way out

[*] posted on 5-12-2016 at 02:06
lead into water - fine, pewter, not so


Something I experienced a long time ago but I caught something on a website that reminded me of it and set me puzzling.

As a kid I used to mess around melting lead and used to pour it into water to make odd shapes. As a 'grown up' ( yeh, right ) I've done the same with silver to make convenient bits for remelting.

Try this with pewter - or quench a pewter mould a little too soon and you're picking bits of metal out of your forehead.

So what's the difference? Why no steam explosion with a metal that melts at 327C or a bit one with one that melts at 170C, is it something to do with the leidenfrost effect?
View user's profile Visit user's homepage View All Posts By User
RogueRose
International Hazard
*****




Posts: 1590
Registered: 16-6-2014
Member Is Offline


[*] posted on 5-12-2016 at 06:15


Quote: Originally posted by Scalebar  
Something I experienced a long time ago but I caught something on a website that reminded me of it and set me puzzling.

As a kid I used to mess around melting lead and used to pour it into water to make odd shapes. As a 'grown up' ( yeh, right ) I've done the same with silver to make convenient bits for remelting.

Try this with pewter - or quench a pewter mould a little too soon and you're picking bits of metal out of your forehead.

So what's the difference? Why no steam explosion with a metal that melts at 327C or a bit one with one that melts at 170C, is it something to do with the leidenfrost effect?


Density different, especially when hot?? was the temp of the water different when doing the pewter? Did you drop the pewter from less distance (lighter weight, less distance = not breaking surface tension as quickly???) IDK, I'm just thinking possibilities..
View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 728
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 5-12-2016 at 07:39



It may have something to do the the Leidenfrost effect.

https://en.wikipedia.org/wiki/Leidenfrost_effect
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 5-12-2016 at 12:38


If you put hot metal in a mould, the metal is trying to get in through the same hole that the steam is escaping from, and that's a problem.
If you just tip hot metal into water there's no problem with any steam that want to just bypassing the metal.
View user's profile View All Posts By User
Scalebar
Hazard to Self
**




Posts: 54
Registered: 6-5-2016
Location: Europe!
Member Is Offline

Mood: Looking for a way out

[*] posted on 6-12-2016 at 00:56


Quote: Originally posted by unionised  

If you just tip hot metal into water there's no problem with any steam that want to just bypassing the metal.


But if you pour pewter straight into water it goes quite emphatically Bang! and sprays everywhere, the same doesn't happen with silver or lead.

The heights would have all been about the same and the water just straight out of the cold tap.
View user's profile Visit user's homepage View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 6-12-2016 at 01:07


Same depth of water?
View user's profile View All Posts By User
violet sin
International Hazard
*****




Posts: 1477
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline

Mood: Good

[*] posted on 6-12-2016 at 01:27


found this: https://www.youtube.com/watch?v=tj7S_DNFgEU
Pouring Molten Metals into Water.

it does show pewter popping at 0:53




View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 728
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 6-12-2016 at 04:47



The dude in the video mentions the Leidenfrost effect a few 10's of seconds into the video. The fact that the pieces will or will not ride down to the bottom of the tank on an insulating layer of water vapour it a major reason why you get different effects.

Tryseeing the effect with a hot smooth bottomed saucepan on a cooker and drop some water into the hot saucepan. At 150C or so water droped into the pan just sizzles. At around 250C the water runs around on the sauspan bottom like mercury for a considerable time.