OK, just received my first piece of glass with a fritted disk, a little 60ml 24/40 Buchner funnel. How do ya clean the frit?



"We believe the knowledge and cultural heritage of mankind should be accessible to all people around the world, regardless of their wealth, social status, nationality, citizenship, etc" z-lib

View user's profile View All Posts By User
BromicAcid
International Hazard
*****




Posts: 3237
Registered: 13-7-2003
Location: Wisconsin
Member Is Offline

Mood: Rock n' Roll

[*] posted on 22-11-2015 at 17:16


Depends on what is on the frit but usually it involves soaking since you can't really carry out too much mechanical manipulation without compromising the integrity and performance of the frit. Usually though the frit is soaked in something that will prove to be volatile so it can be cleaned by being blown or baked dry and not have residue. For example in my quant class we did a quantitative analysis of silver by forming silver chloride. This was collected on a sintered glass frit. For cleaning all of our frits were soaked in concentrated ammonium hydroxide solution before having ammonium hydroxide run through them and oven dried. I have seen nitric used a bit. Piranha even though it doesn't fit the above criteria also gets some use for hard to clean bits. Of course if standard solvents work go for those instead.



Shamelessly plugging my attempts at writing fiction: http://www.robvincent.org
View user's profile Visit user's homepage View All Posts By User
Texium
Administrator
********




Posts: 4544
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: PhD candidate!

[*] posted on 22-11-2015 at 18:25


One time I had to clean mine with chromic acid when I got a bunch of carbon gunk stuck in it. It worked, but since then, I've tried to avoid using it for anything that nasty. Most of the time soaking it in a suitable solvent for whatever it is and then pulling some fresh solvent through it a few times will be sufficient. Strong bases should be avoided though since it can make your frit more porous than it's supposed to be.



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
macckone
International Hazard
*****




Posts: 2160
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 22-11-2015 at 21:20


If there are metal compounds then use nitric acid. It will dissolve everything but sulfates.
For carbon gunk piranha solution is best but never use it if there are metals present that might
form insoluble sulfates. Hydrochloric acid will work on most metal carbonates and hydroxides
but forms insoluble salts with things like silver and lead. Otherwise use a suitable solvent.
Acetone, toluene, hexane, ethanol and water are good examples.
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4544
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: PhD candidate!

[*] posted on 22-11-2015 at 21:29


Yeah, I would have used piranha rather than chromic acid if I had more concentrated peroxide at the time. The chromic acid worked wonders, though it does make a toxic mess that's a pain to clean up which can be avoided with piranha.



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
HeYBrO
Hazard to Others
***




Posts: 289
Registered: 6-12-2013
Location: 'straya
Member Is Offline

Mood: :)

[*] posted on 22-11-2015 at 22:08


You can use fenton's reagent for organic gunk aswell, it is conc. H2O2 and iron sulphate if i remember correctly.
View user's profile View All Posts By User
ave369
Eastern European Lady of Mad Science
****




Posts: 596
Registered: 8-7-2015
Location: No Location
Member Is Offline

Mood: No Mood

[*] posted on 23-11-2015 at 02:49


If there are metals with insoluble sulfates, use chromonitric acid. It is made the same way as chromic acid,but with fuming nitric instead of sulfuric.



Smells like ammonia....