KonkreteRocketry
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 165
Registered: 12-11-2012
Location: Dubai
Member Is Offline
Mood: No Mood
|
|
Can someone guide me from chloride > perchlorate cell?
I got a charger from a broken printer with 20 Volts, and 4.6 Amps.
I can make it around 0.2 Amps per cm2, of water. I have few questions.
I saw Lead Dioxide, Platinum, Manganese Dioxide can be used, will it corrode ? I got plenty powdered Manganese dioxide from carbon batteries, so how
shall i pack it into a like.. piece of solid thing to make it work ?
and. how much NaCl shall i put ?
Also, I saw some chromates and flourides could increase cell efficiency but i have only flourides from tap water..
|
|
hissingnoise
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 3940
Registered: 26-12-2002
Member Is Offline
Mood: Pulverulescent!
|
|
There are many threads here on this subject ─ UTFSE!
|
|
Pyro
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1305
Registered: 6-4-2012
Location: Gent, Belgium
Member Is Offline
Mood: No Mood
|
|
try YT.
Nurdrage has a video on how to make MnO2 electrodes.
also see his videos on electrochemistry
and woelen's page on electrochemistry:
http://woelen.homescience.net/science/chem/exps/miniature_ch...
http://woelen.homescience.net/science/chem/exps/electrolysis...
google:''how to make a perchlorate cell"
you need dichromate
Please try to look for it before you just ask.
all above information is intellectual property of Pyro. ![:D](./images/smilies/biggrin.gif)
|
|
jock88
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 505
Registered: 13-12-2012
Member Is Offline
Mood: No Mood
|
|
You don't need dichromate.
MnO2 electrodes will not make Perchlorate successfully IMO.
|
|
KonkreteRocketry
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 165
Registered: 12-11-2012
Location: Dubai
Member Is Offline
Mood: No Mood
|
|
Thank you, woelen's site is amazing.
|
|
KonkreteRocketry
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 165
Registered: 12-11-2012
Location: Dubai
Member Is Offline
Mood: No Mood
|
|
Ok i got Zinc plates, Tin plates. Does those work?
Btw if i use a 20 Volt circuit , does it do anything ? why does those places mention 5 volt, does the volt really matter a lot ?
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7988
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
The voltage really matters a lot. Don't use 20 volts! The reaction itself requires a very specific voltage (each half-reaction on the anodes and
cathodes requires a specific voltage) and added to that, there is overpotential (e.g. due to conversion from liquid to gas) and there is ohmic
resistance in the cell. The latter causes conversion of electric power to heat. If you use 20 volts, then
1) your cell will run extremely hot
2) you may destroy your power supply, unless it is a very powerful one or has good shortcircuit protection
3) you will destroy your anode
4) you will have all kinds of undesirable side-reactions which do not produce chlorate.
You can use a higher than 5 volts power supply, but then you need to add series resistors for limiting the current. But if you use 20 volts, then 90%
of your power is converted to heat and you will get red hot resistors!
|
|
KonkreteRocketry
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 165
Registered: 12-11-2012
Location: Dubai
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by woelen ![](images/xpblue/lastpost.gif) | The voltage really matters a lot. Don't use 20 volts! The reaction itself requires a very specific voltage (each half-reaction on the anodes and
cathodes requires a specific voltage) and added to that, there is overpotential (e.g. due to conversion from liquid to gas) and there is ohmic
resistance in the cell. The latter causes conversion of electric power to heat. If you use 20 volts, then
1) your cell will run extremely hot
2) you may destroy your power supply, unless it is a very powerful one or has good shortcircuit protection
3) you will destroy your anode
4) you will have all kinds of undesirable side-reactions which do not produce chlorate.
You can use a higher than 5 volts power supply, but then you need to add series resistors for limiting the current. But if you use 20 volts, then 90%
of your power is converted to heat and you will get red hot resistors! |
Wow ok, that is lot more than expected. Do you know if i could use Zinc or tin plates for electrolysis ?
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
You could hook up 4 cells in series to get 5 volts across each one, assuming they are identical. I don't think zinc plates would work very well (they
would corrode), but tin might.
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7988
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
Zinc does not work as anode, nor does tin. Really, you only have very few options:
- platinum, useful for making perchlorate from chlorate. Do not use for making chlorate from chloride!
- MMO, perfect for making chlorate from chloride, not useful for making perchlorate.
- PbO2, can be used for making perchlorate, to some extent also suitable for making chlorate.
- graphite, useful for making chlorate from chloride, but messy (slowly erodes, giving black crud in your solution).
Metals like tin, lead, zinc, aluminium, titanium, silver, tungsten, and so on either quickly dissolve or passivate. MMO anodes are affordable, PbO2
anodes apparently can be made at home, but I have no experience with that and this is not something for the unexperienced, due to the need to work
with large amounts of very toxic chemicals. Making perchlorates at home hardly is an option, unless you intend to use a large amount of them. I only
needed small quantities for little experiments and then it is better to simply buy them. If you are into pyrotechnics and use kilos per year, then it
may be worth investing in platinum anodes and use those to make perchlorate from chlorate.
|
|
KonkreteRocketry
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 165
Registered: 12-11-2012
Location: Dubai
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by woelen ![](images/xpblue/lastpost.gif) | Zinc does not work as anode, nor does tin. Really, you only have very few options:
- platinum, useful for making perchlorate from chlorate. Do not use for making chlorate from chloride!
- MMO, perfect for making chlorate from chloride, not useful for making perchlorate.
- PbO2, can be used for making perchlorate, to some extent also suitable for making chlorate.
- graphite, useful for making chlorate from chloride, but messy (slowly erodes, giving black crud in your solution).
Metals like tin, lead, zinc, aluminium, titanium, silver, tungsten, and so on either quickly dissolve or passivate. MMO anodes are affordable, PbO2
anodes apparently can be made at home, but I have no experience with that and this is not something for the unexperienced, due to the need to work
with large amounts of very toxic chemicals. Making perchlorates at home hardly is an option, unless you intend to use a large amount of them. I only
needed small quantities for little experiments and then it is better to simply buy them. If you are into pyrotechnics and use kilos per year, then it
may be worth investing in platinum anodes and use those to make perchlorate from chlorate. |
I have MnO2, which ive heard is good, but its in powdered form, how shall i turn it into a good electrode ?
|
|
elementcollector1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline
Mood: Molten
|
|
I have MnO2, which ive heard is good, but its in powdered form, how shall i turn it into a good electrode ?[/rquote]
You'll need nitric acid, a titanium electrode, a pipette and a hotplate. Given that manganese nitrate decomposes upon heating to MnO2, I'll let you
work out the rest.
Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7988
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
I don't think it is easy to make an electrode from powdered MnO2. Similarly, I have powdered PbO2 but making an electrode from that is not possible.
Probably you need to start from a manganese(II) salt in solution and use electrolysis at precisely controlled pH using precisely controlled current
density in order to electrolytically oxidize the Mn(2+) to MnO2. A similar process is used for making PbO2 anodes from solutions of Pb(NO3)2. This
process, however, is very hard to control. You easily get badly adhering layers or powdery deposits on the anode. I think that the MnO2-process is not
better than the PbO2-process. Hard to control and extremely difficult to get something useful.
|
|