Tutorial for making a miniature chlorate cell
Quite a lot of tutorials are present on the Internet for building chlorate cells, using all kinds of anodes and all kinds of big containers for making
hundreds of grams per day or even almost 1 kilo per day. That kind of cells are big, need a power supply capable of delivering tens of amperes and
need big MMO anodes and equally big cathodes.
For the home chemist, who just wants 50 to 100 grams of KClO3 for nice fire-demos or small-scale syntheses the construction of those big cells may
look rather intimidating.
I made a very small 100 ml cell, which allows one to make 30 grams of KClO3 per day and which can be operated from a simple fixed 5 volt power supply,
which only needs to be capable of delivering 5A (the cell itself takes only 3 to 4 A, but using a 5 A power supply gives some headroom and allows for
tolerances in construction of the cell). Cost of the cell only is $30, excluding the power supply.
http://woelen.homescience.net/science/chem/exps/miniature_ch...
The potassium chlorate, obtained from this cell is perfectly white, it really is white like snow. For making this cell, I used specially made anodes,
made by our own sciencemadness member Swede. See the webpage for more info.
[Edited on 24-9-10 by woelen]
|
|
aonomus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 361
Registered: 18-10-2009
Location: Toronto, Canada
Member Is Offline
Mood: Refluxing
|
|
Link to the actual project page: http://woelen.homescience.net/science/chem/exps/miniature_ch...
|
|
mr.crow
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 884
Registered: 9-9-2009
Location: Canada
Member Is Offline
Mood: 0xFF
|
|
Great article! Its a shame about the bromate not working.
I am going to try making a chlorate cell this weekend using a normal scale eBay anode.
Double, double toil and trouble; Fire burn, and caldron bubble
|
|
Contrabasso
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 277
Registered: 2-4-2008
Member Is Offline
Mood: No Mood
|
|
The electrodes are critical and Swede has done lots of research into materials sizes and types to get good cell performance. He has shared his
research so please don't waste the shared wisdom.
Some people found that glass containers were not best suited, and also found that power supply interruptions were very bad for the cell integrity.
However this was found in larger cells running 50 to 100 amps into a large enough cell to run around the 75C mark.
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7990
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
Power supply interruptions for longer time indeed are very bad. A short interrupt for a few tens of seconds for topping up liquid level does no real
harm, provided one uses titanium cathodes.
I did not know of the problem with glass. I myself don't have any problems with this, but I'll change the page and mention the problem with glass when
larger cells are used. I'm quite sure this has to do with high pH, which leads to dissolving some of the silicate in the glass, which can settle at
the electrodes. I, however, never allow my electrodes to get dry. I take them out of the glass jar and immediately transfer them to a beaker full of
tap water. That probably greatly helps preventing the buildup of a silicate layer on the electrodes.
I also did another experiment. I have been running the cell, but now without any cooling. The glass container became so hot that I could not bear
touching it. But the current efficiency is better. Already 18 hours after power on, there was a quick transition of just a little oxygen production at
the anode to very fast oxygen production at the anode. This means that almost chloride has been used up at that point and that the cell simply
decomposes water (MMO anodes don't make perchlorate, they simply make oxygen at the anode). In order to test my hypothesis I added a few grams of KCl,
dissolved in a few ml of boiling water. Almost immediately after adding this KCl, the production of gas at the anode ceased, until after an hour or so
the production of gas at the anode was quite fast again.
So, running the cell really hot is tempting from a point of view of current efficiency, but it also puts more strain on the anode and the overall cell
construction. For next runs, I'll use some cooling again, I just did this single experiment to see how much of a difference it makes.
[Edited on 25-9-10 by woelen]
|
|
mnick12
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 404
Registered: 30-12-2009
Location: In the lab w/ Dr. Evil
Member Is Offline
Mood: devious
|
|
Now I know this is not directly related, but it is similair and does not deserve its own thread. Regular bleach is about 5% NaOCl and often times has
detergents mixed in, and pool chlorinator is usually about 16% NaOCl with lots of impurities. And as you all know electrolysis of NaCl solutions first
forms NaOCl which dissasociates into NaClO3 and more NaCl. So I am interested in modifying a chlorate cell to produce concentrated NaOCl solutions.
How would I go about doing this? Would simply keeping the solution cold produce hypochlorite, or are there other factors? I have made a few pounds of
sodium and potassium chlorate from a Co3O4/NiO coated Ti anode, but I am not quite sure how to produce the hypochlorite alone.
Oh and the reason why I am asking, is I plan on using the hypochlorite for various organic oxidations as it seems to be cheap and has good yields.
Thanks!
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7990
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
The web page is updated. The remark of Contrabasso on the use of a glass bottle is put in the webpage and also the results of the third run without
cooling are mentioned in the webpage.
@mnick12: I do not think that making hypochlorite is possible by simply keeping the cell cold. As I wrote in my webpage, when the hypochlorite cannot
be converted to chlorate in the liquid (either by low temperature, or by too high pH), then hypochlorite ions are oxidized to ClO radicals and these
recombine and react with water to give chlorate, chloride and oxygen. So, when you keep the cell cold you also get chlorate, albeit at a lower current
efficiency.
If you really want to make hypochlorite of decent purity, then I think that a much better way is to bubble Cl2 through a solution of NaOH until no
more Cl2 is absorbed. For stability you then can add a little amount of NaOH again in order to bring up the pH, such that all hypochlorite is present
as ClO(-) and not as HOCl.
|
|
12AX7
Post Harlot
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
I discovered the same problem with bromate. I once attempted to use a platinized titanium anode, which promptly resulted in a large mess of white
goo.
Tim
|
|
metalresearcher
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 737
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Ten years ago I made some KClO3 with success from diet salt (2 parts KCl + 1part Nal), it is rather pure.
See on www.metallab.net/KClO3 .
But thiis method without carbon anodes will be better.
|
|
Contrabasso
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 277
Registered: 2-4-2008
Member Is Offline
Mood: No Mood
|
|
The industrial process for Perc is in two parts, First the chloride is electrolysed to chlorate, this is then purified. In a separate cell chlorate is
electrolysed to perchlorate using precious metal electrodes. Think big batches and very big currents!
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7990
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
Last weekend I used my miniature cell for making CsClO3. The key to success with CsClO3 is not to use too concentrated solutions.
CsClO3 can be made from CsCl just like KClO3 can be made from KCl. With KCl you have to make a more or less saturated solution, with CsCl that will
lead to coverage by crystals and blocking of the electrodes.
A good concentration is to take 40 grams of CsCl and dissolve that in water, such that 100 ml of solution is obtained. This solution can be
electrolysed until the current drops to just a fraction of the initial current. At that point more than 90% of all CsCl is converted to CsClO3.
There are more differences with KCl. You cannot simply add some K2Cr2O7 to the solution of CsCl. It gives a nasty sticky precipitate of Cs2Cr2O7,
which does not dissolve. Instead, you must dissolve just a tiny amount (e.g. 20 mg) of K2Cr2O7 in a few ml of water and add this solution to a hot
solution of CsCl and stir. The resulting liquid then is yellow.
The following procedure can be used to make CsClO3. I have done it a few times and it works like a charm:
- Take 40 grams of CsCl and add 60 ml of very hot water. Dissolve all of it and if necessary, filter the solution.
- Dissolve a tiny amount of K2Cr2O7 in a few ml of water. Bring this to a boil.
- Add the boiling hot solution of K2Cr2O7 to the hot solution of CsCl and stir.
- Top up to 100 ml and stir to make the solution homogeneous.
- Start electrolysis and measure the starting current.
- Assure that the cell remains rather hot. If the electrolysis process does not provide enough heat, then use external heating. However, usually the
process provides enough heat from itself.
- Keep on electrolysing until the current has dropped to just a fraction of the starting current. This may take a long time, depending on the initial
current. At a current of 1 A this may take two full days. During the process it might be necessary to top up the cell with hot water. Only do this
when the volume drops below 80 ml. Then top up to 90 ml.
- If no external heat is applied and the cell runs sufficiently hot from itself, then you can also notice the end of the process by cooling down of
the cell.
- At the end of the process there will be a lot of crystal mass at the bottom.
- Disconnect the electrodes and allow the cell to cool down slowly to room temperature.
- After cooling down, put in the fridge to allow further cool down to 0 C or even colder (but it should not freeze).
- Decant the yellow liquid from the crystal mass as good as possible.
- Take a heap of paper tissue and put a coffee filter on it. Put the crystal mass on the filter and allow liquid to sock in the filter and paper
tissue. Repeat this step one or two times.
- Recrystallize from 50 ml or so of boiling water. Assure that ALL crystals dissolve. Add portions of 10 ml of water until all crystals have
dissolved.
- Allow to cool down, decant liquid, make dry on filter paper and tissue, and then rinse with ice cold water and dry another time on a fresh filter
and paper tissue.
- Give a final dry at a warm place for one day (e.g. on a heating radiator for one day).
Yield of this procedure: 80%, based on CsCl, approximately 40 grams of CsClO3.
If all the rinsing water and the yellow liquid are kept, then the Cs in that also can be recovered partially. In total, I had 140 grams of CsCl
available for this experiment. I made 145 grams of CsClO3 from that and from all the rinse water and so on, I also recovered approximately 20 grams of
CsClO4 (by treating that with a solution of NaClO4). So, in total I lost approximately 10% of all Cs, most of that being lost in the coffee filters
and the liquid, absorbed by the paper tissue. It is fun to let the coffee filters dry and then light them with a cigarette lighter. The burning of the
coffee filters is quite spectacular ![:)](./images/smilies/smile.gif)
[Edited on 17-4-12 by woelen]
|
|
12AX7
Post Harlot
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
How's the flame color, do we get a video?
|
|
woelen
Super Administrator
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 7990
Registered: 20-8-2005
Location: Netherlands
Member Is Offline
Mood: interested
|
|
I tried making a video of the burning of a mix of CsClO3 and sulphur and also one of burning a mix of KClO3 and sulphur. The resulting video is
disappointing and does not render the nice colors which I can see. The flame simply is over-exposed and white. I'll have to wait for a bright day and
make a video on that day. My problem is that the camera takes average brightness and while the background still looks OK, the flame is way too light.
Unfortunately, over here the days are very short now (I go to work in darkness and come home in darkness), so the bright day must be a weekend day.
The flame color of a CsClO3/S mix is blue/purple. It is not purely blue. The flame color of a KClO3/S mix is more pinkish, but it also depends on the
amount of sulphur in the mix. When excess sulphur is used, then the color is more blue.
My idea is to make a mix of CsClO3 and S and a mix of KClO3 and S. Then CsClO3/S mix is put in the form of a line (5 cm length, 5 mm width) and
adjacent to this the KClO3/S mix is put in the form of a similar line. Then I light the total line on one side. Then you first see the color of the
burning of the CsClO3/S mix and then you see that color change to the color of a burning KClO3/S mix. I also might add a line of Ba(ClO3)2/S mix to
this (my next project is making Ba(ClO3)2 from BaCl2, I am in the process of acquiring appr. 1 kilo of BaCl2).
[Edited on 8-11-10 by woelen]
|
|
12AX7
Post Harlot
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
It might help to burn the compositions in front of a white screen, to reflect the light and brighten the scene.
Tim
|
|
Arthur Dent
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 553
Registered: 22-10-2010
Member Is Offline
Mood: entropic
|
|
Sorry to revive this antique thread but I have a question for Woelen about the material used for this cool cell project.
Being a cheapskate, I was wondering about the Titanium / MMO electrodes. I have secured a good-sized sheet of metallic titanium (top cover of an old
G4 powerbook). So my titanium cathode is good to go.
Now about the MMO anode, could I use instead Platinum wire? I happen to have two spools of "Platinum alloy" wire and was thinking of wrapping a
lenght of it on a glass canule...
I imagine that the reason Titanium isn't used as the anode material is that it's attacked by the electrolysis and generates Titanium Chloride?
And if I recall, carbon anodes are very good and inert but have this unfortunate tendency of slowly disintegrating and mixing carbon residue and
bonding agents with the resulting chlorate...
Anyway, just a few vague questions on the anode material. I was thinking of trying out this experiment and since I have a fair amount of Ti and a good
power supply, my last hurdle was to find an alternative to the purchase of a ready to use mixed-metal-oxide anode.
I have about 400 g of Potassium Chloride to use in my future cell so I have many of the main ingredients to get this project going.
Robert
--- Art is making something out of nothing and selling it. - Frank Zappa ---
|
|
cyanureeves
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 744
Registered: 29-8-2010
Location: Mars
Member Is Offline
Mood: No Mood
|
|
arthur i know you summoned woelen in specific but i think titanium as an anode just stops conducting altogether after a while.nurdrage does that mmo
with the stuff made from battery crud. i have gotten as far as making the battery crud manganesee sulfate stuff but stopped because i still needed
cobalt nitrate for the first coat.you got two spools of platinum wire? wow i wouldve tried it out with a two inch piece for sure and i'm sure that
even though its platinum alloy its still expensive. i also think i will invest on some mmo electrodes or plated ones. well i will wait on woelens
response to you as well.
[Edited on 14-8-2011 by cyanureeves]
|
|
m1tanker78
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 685
Registered: 5-1-2011
Member Is Offline
Mood: No Mood
|
|
I've never had a problem filtering out the carbon crud from gouging rods. Each lasts many dozens of hours, or hundreds. Maybe I'm missing something
but graphite rods are the perfect solution for a HC who wants to make chlorate on the cheap, seems to me.
Tank
|
|
cyanureeves
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 744
Registered: 29-8-2010
Location: Mars
Member Is Offline
Mood: No Mood
|
|
hey tank.i am using carbon rods from a 6 volt battery but i saw some graphite rods on ebay and thought about buying one . are graphite rods way better
than the carbon rods? i googled how to make chlorate and a fella there called 6volt battery rods, graphite. this is not correct is it?
|
|
m1tanker78
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 685
Registered: 5-1-2011
Member Is Offline
Mood: No Mood
|
|
Reeves, I've never tried with battery carbons. I use 'graphite' gouging rods although I think that's also a misnomer. By my eyeball, they seem to be a
mixture of graphite, carbon, probably clay and who knows what else. I can make 'pencil' marks on a rough surface with some difficulty. They even hold
up pretty well in my sodium cells (consumable item).
Check your local welding supply stores to see what sizes and pricing they offer. Virtually all have copper cladding that's easy to remove in a dummy
chlorate cell. Again, the little bit of stuff that does shear off is very easy to filter with frit or similar.
Real graphite is very soft and easily marks almost any surface. I can't say from experience if these graphite rods provide any real advantages over
gouging carbons. If the price is right, go for it.
Tank
|
|
dann2
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1523
Registered: 31-1-2007
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by cyanureeves ![](images/xpblue/lastpost.gif) | .........battery crud. i have gotten as far as making the battery crud manganesee sulfate stuff but stopped because i still needed cobalt nitrate for
the first coat........
[Edited on 14-8-2011 by cyanureeves] |
You don't need Cobalt Oxide (from Cobalt Nitrate) as a first coat. Mn Oxide on it's own is fine. The Cobalt Oxide may even be a disadvantage. Cobalt
Oxide lasts only a short time in a Chlorate cell, even less time in a Perk. cell. Use any spare money, time or energy that you may have putting on
extra MnO2 coats.
Dann2
|
|
cyanureeves
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 744
Registered: 29-8-2010
Location: Mars
Member Is Offline
Mood: No Mood
|
|
thanks tank, thanks dann2.
|
|
Arthur Dent
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 553
Registered: 22-10-2010
Member Is Offline
Mood: entropic
|
|
I do have some graphite rods (I picked-up a box when I was a projectionist at a movie theatre) so I might try to use the combination of a Titanium
cathode and a Graphite anode.
As for the container, I was thinking of using Silicone caulking to seal the electrode contacts and the glass vent tube on the top cover for a really
airtight container and drive the resulting gases through a vinyl tube. Has anyone tried Silicone caulking, the bathroom tile joints kind? Does it
resist the temperatures generated by the cell?
The cool part about graphite rods instead of carbon battery rods is that these graphite rods are extra long and when one starts to shorten because of
degradation, you just push it a little further down in the solution. (the principle of the carbon arc light in these antique movie projectors, except
it was a notorised insertion system that slowly pushed the rod for optimal arc).
Of course the platinum wire would be best but i've been scratching my head as how to use it effectively in a cell by wrapping it around something
inert and heat-resistant.
Just thinking aloud. it would be great if I could use the materials I have at my disposal, it's just a bit of mechanical engineering I have to come up
with...
Robert
[Edited on 16-8-2011 by Arthur Dent]
--- Art is making something out of nothing and selling it. - Frank Zappa ---
|
|
sternman318
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 121
Registered: 21-4-2011
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Arthur Dent ![](images/xpblue/lastpost.gif) |
Of course the platinum wire would be best but i've been scratching my head as how to use it effectively in a cell by wrapping it around something
inert and heat-resistant.
|
Scroll down to the section on electrodes
http://woelen.homescience.net/science/chem/exps/KBrO3_synth/...
|
|
m1tanker78
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 685
Registered: 5-1-2011
Member Is Offline
Mood: No Mood
|
|
Robert, I've had good results with rubber grommets. If you want to mechanically fix the electrodes to the cell, liquid nails is the best I've used so
far. JB weld (actually, most 2-part epoxy) won't stick worth a damn to plastic unless it's pre-conditioned.
If you keep the temp, pH, chloride, etc. in check, your gouging rod(s) will complete several batches without having to readjust the depth. I rigged up
a crude electrolyte drip delivery system and it worked great at keeping the cell running at optimized levels.
The crude liquor looks like crap but once run through a fine frit filter, you have crystal clear, yellow-tinted Chlorate liquor ready to convert to
potassium chlorate (if desired).
Must be nice having platinum wire at your disposal. ![:D](./images/smilies/biggrin.gif)
Tank
|
|
cyanureeves
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 744
Registered: 29-8-2010
Location: Mars
Member Is Offline
Mood: No Mood
|
|
dann2 is manganese dioxode really enough and no need for cobalt nitrate? i would rather bake the manganese on than electroplate the anode because
nurdrage's flaked off.
|
|
Pages: