Author: Subject: Separating Bismuth Powder From Aluminum
mesanaw
Harmless
*




Posts: 10
Registered: 29-10-2016
Member Is Offline

Mood: No Mood

[*] posted on 29-10-2016 at 07:45
Separating Bismuth Powder From Aluminum


I am trying to extract bismuth from Pepto Bismo using the HCL and aluminum procedure, but I ended up with a pile of bismuth powder mixed in with aluminum. The aluminum pieces are too small and brittle to manually remove and I think around 40% of the powder is aluminum.
Does anyone have any suggestions on how to separate the two metals so that I end up with mostly bismuth?
Thanks.
View user's profile View All Posts By User
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 29-10-2016 at 07:57


Maybe Sodium Hydroxide to dissolve the Al?
I dont know what it will do to the bismuth though
View user's profile View All Posts By User
pinkamena
Harmless
*




Posts: 2
Registered: 23-8-2016
Member Is Offline

Mood: No Mood

[*] posted on 29-10-2016 at 09:15


You could just throw the whole mixture into hydrochloric acid, aluminium will dissolve because it's electropotential is below that of hydrogen (Al3+ + 3e- > Al : -1.7V), and bismuth will remain because it's electropotential is above that of hydrogen (Bi3+ + 3e- > Bi : +0.4V).
View user's profile View All Posts By User
mayko
International Hazard
*****




Posts: 1218
Registered: 17-1-2013
Location: Carrboro, NC
Member Is Offline

Mood: anomalous (Euclid class)

[*] posted on 29-10-2016 at 09:49


Did you shred the aluminum? I've seen some preps do this but I've precipitated bismuth just fine with an aluminum foil sheet corrugated into a fan, with minimal aluminum contamination



al-khemie is not a terrorist organization
"Chemicals, chemicals... I need chemicals!" - George Hayduke
"Wubbalubba dub-dub!" - Rick Sanchez
View user's profile Visit user's homepage View All Posts By User
mesanaw
Harmless
*




Posts: 10
Registered: 29-10-2016
Member Is Offline

Mood: No Mood

[*] posted on 29-10-2016 at 12:02


I just stirred the solution with a large piece of aluminum and then let it rest in the container. I'm going to try washing it with dilute HCL and hopefully that will work.

It worked perfectly. I have some really clean-looking powder thanks everyone!

[Edited on 29-10-2016 by mesanaw]
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 31-10-2016 at 06:30


The real trick is turning that powder into a solid ingot of metal! Because of its high surface area, it oxidizes to yellow bismuth(III) oxide instead of melting when heated. I tried a few tricks to get it to melt but never could. Now that I have an argon cylinder, it might be worth looking into again.
View user's profile Visit user's homepage View All Posts By User
elementcollector1
International Hazard
*****




Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline

Mood: Molten

[*] posted on 31-10-2016 at 07:39


I managed to do it with cadmium powder and copious amounts of NaOH flux, so it should be possible.



Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
View user's profile View All Posts By User
Deathunter88
National Hazard
****




Posts: 517
Registered: 20-2-2015
Location: Beijing, China
Member Is Offline

Mood: No Mood

[*] posted on 31-10-2016 at 10:44


Here is a video of Nile Red getting bismuth metal into an ingot from powder that he extracted from pills. He says that strong heating of the bismuth oxide will decompose it back into bismuth metal and oxygen.

https://www.youtube.com/watch?v=grpSfjUImUs
View user's profile View All Posts By User