Author: Subject: Proper electrode material for arc melting steel
metalresearcher
National Hazard
****




Posts: 732
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 16-9-2023 at 10:06
Proper electrode material for arc melting steel


Sometimes I melt (stainless) steel using a DC arc welder with carbon rods. But after melting, the steel gets brittle as it absorbs carbon and transforms to cast iron. Once I used thick steel wire embedded in refractory cement ending in the bottom of the cavity where the steel is to be melted. That works, I connect the steel wire to the anode and use a carbon rod as cathode. So, when the steel is molten, the steel bath acts as anode. But, yet the metal gets brittle as well.
Might be tungsten rods can be a solution, but W also oxidizes quickly at steel melt temperatures.
Commercial EAF melt shops in steel industry use C rods as well, but they have much better control over the composition of the steel bath.
Does anybody have ideas / experiences ?
View user's profile View All Posts By User
mysteriusbhoice
Hazard to Others
***




Posts: 477
Registered: 27-1-2016
Member Is Offline

Mood: Became chemistry catboy Vtuber Nyaa

[*] posted on 16-9-2023 at 14:57


if you have inert gas you can probably use tungsten as your electrode
View user's profile Visit user's homepage View All Posts By User
Rainwater
National Hazard
****




Posts: 821
Registered: 22-12-2021
Member Is Offline

Mood: indisposition to activity

[*] posted on 17-9-2023 at 04:10


O2 is blown into the melt which produces CO that bubbles out of the mix. Any Fe that reacts first to form oxides will be reduced back into metal by the carbon content.
Its a secret process for each manufacturer so the exact details are hard to obtain and are batch dependent




"You can't do that" - challenge accepted
View user's profile View All Posts By User
Twospoons
International Hazard
*****




Posts: 1289
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline

Mood: A trace of hope...

[*] posted on 17-9-2023 at 13:01


Are you sure its not just the fact that its cast thats resulting in brittleness? Typical steels get tougher through hot or cold working, then tempering. You dont get that with a casting.