Author: Subject: More on PbO2 electrodes
testimento
Hazard to Others
***




Posts: 351
Registered: 10-6-2013
Member Is Offline

Mood: No Mood

[*] posted on 26-2-2014 at 16:29


Does anyone have knowledge or experience on lead acetate electroplating PbO2 on graphite?
View user's profile View All Posts By User
UncleJoe1985
Hazard to Self
**




Posts: 88
Registered: 30-9-2008
Location: Sunnyvale, CA
Member Is Offline

Mood: No Mood

[*] posted on 23-4-2015 at 02:32
use tin as a substrate?


Quote:
Does anyone have knowledge or experience on lead acetate electroplating PbO2 on graphite?


I've made 2 attempts using the easier to obtain acetate.
The results are extremely crude due to not controlling the parameters to be within spec.

1st attempt (simple proof of concept):
coating was extremely flaky and crystal like, with minimal adhesion (could easily wipe it off)

Not surprising since I used no agitation to remove bubbles, room temperature, current density was too high (15mA/cm2), used too much CuSO4 that it seemed to displace the lead from solution, cathode current density too low (why does it recommend it to be 2x the anode current density - to prevent lead from plating out?)

2nd attempt - this time I used a heat gun to heat the solution and provide slight agitation

Result:
No longer flaky and better adhesion after drying, but very spongy instead of solid. I measured the resistance between 2 points 1cm apart and it was ~200 ohms. The graphite rod I used was 10cm x 1cm.

Next: use lower current density, do better job of removing bubbles, use less CuSO4


View user's profile View All Posts By User
UncleJoe1985
Hazard to Self
**




Posts: 88
Registered: 30-9-2008
Location: Sunnyvale, CA
Member Is Offline

Mood: No Mood

sad.gif posted on 10-5-2015 at 05:52


OMG, I'm an idiot for using CuSO4 :(

That would ruin the plating solution by precipitating the lead out as sulfate! And I used so much CuSO4.

I was wondering what all that white crud at the bottom was. Guess I'll try again with copper acetate.

I think I intuitively understand why copper plates out before lead at the cathode. To explain it in simple physics principles, copper is less reactive than lead, meaning it's harder to ionize. That would mean the Cu ions have a higher electrostatic potential energy. Since the lowest potential energy state is favored, the electrons go to Cu2+.

But what about at the anode? Does oxidation of copper to copper oxides compete with Pb2+ + 2 H2O -> PbO2 + 4 H+ + 4e- (correct me if I'm wrong)

Can anyone point me to the relevant electrode potentials involved?


[Edited on 10-5-2015 by UncleJoe1985]
View user's profile View All Posts By User
Jstuyfzand
Hazard to Others
***




Posts: 166
Registered: 16-1-2016
Location: Netherlands
Member Is Offline

Mood: Learning, Sorta.

[*] posted on 2-4-2016 at 14:29


What do you all think of this video? Seems pretty good!
https://www.youtube.com/watch?v=bZMWEYiTtso
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1457
Registered: 2-9-2014
Location: Tel Aviv University
Member Is Offline

Mood: old jew

[*] posted on 15-7-2016 at 12:44


Is possible pure PbO2 pressed ? Pressure 12 000 Kg on cm2. And making 10 cm long rod from pure PbO2 ? Diameter 15 mm. How is electric conduction - resistance for PbO2 ? And If is impossible pressed pure PbO2, is possible adding some material for increase solid ? For example, 7% nitrocellulose is confirmed as very good solid - agent. For any fine-powder materials. What using 5% epoxide ? Or some different additivum for increase solidity? Anode will be for prepare NaClO4, of course. Will be nitrocellulose do it problems ? Thanks, ...LL...:cool:
View user's profile View All Posts By User
PHILOU Zrealone
International Hazard
*****




Posts: 2894
Registered: 20-5-2002
Location: Brussel
Member Is Offline

Mood: Bis-diazo-dinitro-hydroquinonic

[*] posted on 17-7-2016 at 04:38


Quote: Originally posted by Laboratory of Liptakov  
Is possible pure PbO2 pressed ? Pressure 12 000 Kg on cm2. And making 10 cm long rod from pure PbO2 ? Diameter 15 mm. How is electric conduction - resistance for PbO2 ? And If is impossible pressed pure PbO2, is possible adding some material for increase solid ? For example, 7% nitrocellulose is confirmed as very good solid - agent. For any fine-powder materials. What using 5% epoxide ? Or some different additivum for increase solidity? Anode will be for prepare NaClO4, of course. Will be nitrocellulose do it problems ? Thanks, ...LL...:cool:

I don't know for the pressed PbO2 stick/rod and properties...

What I know:
Nitrocellulose will be unstable cement because in basic media (what the cell will increase (bleach is already stongly basic for stability and to avoid toxic Cl2, Cl2O, ClO2 gas generation)) it will be hydrolysed into cellulose...thus setting NO3(-) free (good or bad?)...
Now, I don't know how cellulose behaves into a bleach-chlorate-perchlorate cell...but that's easy to find out (by experiment))...will it remain integer or will it be chewed/schreded into pieces?
The following document:
Cellulose solvents and dissolution medias seems to mention that NaOH (7-10%) is able to dissolve cellulose...
You can also make Sweitzers type of solvent or Cellulose xanthan and the precipitate the cellulose into the PbO2 rod...maybe you could work with cellophane another form of polymerized cellulose.

Epoxyde should remain stable into basic media...only into strongly acidic media it would be hydrolysed (but acidic is uncompatible with bleach...so should be OK).





PH Z (PHILOU Zrealone)

"Physic is all what never works; Chemistry is all what stinks and explodes!"-"Life that deadly disease, sexually transmitted."(W.Allen)
View user's profile View All Posts By User
Laboratory of Liptakov
International Hazard
*****




Posts: 1457
Registered: 2-9-2014
Location: Tel Aviv University
Member Is Offline

Mood: old jew

[*] posted on 17-7-2016 at 07:19
PbO2 anode


Thanks, epoxide as binder can be maybe a good material. During next study is clearly , that surface must be perfectly, without micro holes in the surface. Thus, electro deposition on some substrate is necessary process. Unfortunately. Still more thanks, I making it on this. ..LL...:cool:
View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 820
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 11-1-2017 at 10:39


Lead dioxide anode for sale 30 dollars + shipping

read all about it here

http://www.amateurpyro.com/forums/topic/1629-making-potassiu...



leadioxide.jpg - 19kB
View user's profile View All Posts By User
ecos
Hazard to Others
***




Posts: 464
Registered: 6-3-2014
Member Is Offline

Mood: Learning !

[*] posted on 12-2-2017 at 05:23


Quote: Originally posted by yobbo II  
Lead dioxide anode for sale 30 dollars + shipping

read all about it here

http://www.amateurpyro.com/forums/topic/1629-making-potassiu...



what is the thickness of the coating and the anode size?
View user's profile View All Posts By User
Ziggy4
Harmless
*




Posts: 1
Registered: 19-7-2017
Member Is Offline

Mood: No Mood

[*] posted on 19-7-2017 at 11:24


I have a thought that should apply to this thread. Upon my own interest in perchlorate synthesis, and reading this thread, and ideas about using inert plastics and solvents like MEK etc. to create a slurry of lead dioxide then coating some metallic substrait with it to use as an anode has me thinking that possibly softening plexiglass with solvent and esssentially rolling it in PbO2, then electroplating more of it onto it electrolytically would work too. I also read Sweede's blog about the subject, and his offset weighted agitator to facilitate degassing of the electrode. He was using surficants to help with that too. How about using an ultrasonic cleaning tank as the plating bath to agetate and mix the entire soln? I found a couple studies on this method and one that uses a probe to deliver the ultrasonic energy past the electrode perpendicularly. The results were very favorable.
http://www.sciencedirect.com/science/article/pii/S0009250914...
And http://www.sonochemistry.info/electro.htm
Hopefully I didn't step out of line here since I am brand new to this forum, and very interested in many topics here. I just couldn't hold back on this possibility though and so I joined in order to make this post and see what you all think.
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 18-3-2018 at 06:44


Ladies and gentlemen!

Allow me to present the first practical results regarding the realization of an idea I have had sprouting around in my head for the better part of the current decade: "electrodeposition of lead dioxide coatings with soluble Pb+2 generated in situ"

As we are well aware, the lead dioxide electrodeposition process tends to be rather inconvenient due to the coupious amounts of soluble lead componds involved (lead nitrate, acetate or plumbate). Not having the personal inclination towards engaging in close contact with these substances during the electrolyte preparation stage, I had the idea of starting from more benign materials and forming the required soluble lead in the electrodeposition process as a byproduct.

The starting materials being : metallic lead, ammonium nitrate, nitric acid

The process itself would be conducted in a cell having ammonium nitrate solution acidified with nitric acid as the electrolyte and three metallic electrodes submersed into the liquor. Two of the electrodes would be metallis lead and one the substrate on which the electrodeposition of lead dioxide shall take place.

The electrodes would have a current divider constructed between them to separate the required electrochemical processes to the respective electrodes and the cell would be driven in a "semi alternating current" mode. The latter is accomplished by a mosfet H bridge, wich allows to reverse the currents and redirect the processes onto different electrodes.


DSCF1603.JPG - 1MB

DSCF1604.JPG - 960kB
Fig.1 the simplified illustration of the process and setup

The idea is to dissolve lead from Pb electrode nr 1 during period t1 by routing current from the h-bridge output through the current divider diodes to electrodes 1 and 3 and thus creating a resident net concentration of soluble lead in the cell liquor. This takes place at an uncontrolled current density as the anodic solution of lead does not need to be currnt controlled in this application.
After that the current from the h-bridge output is reversed and routed again through the cell during a period of t2, but the current divider giving it a different path this time: the central substrate electrode nr 2 being anodically porarised against electrode nr 1.
Thus partial electrodeposition of lead dioxide should start on the central inert substrate electrode, accompanied by the cathodic deposition of metallic lead on electrode nr 1 from which the lead was originally dissolved in previous period.
The current density is being reduced during this process by the 270 ohm resistor in the current divider, as this step needs to be conducted at low currents (in vincinity of 3mA/cm2) to minimize internal stresses in the formed PbO2 layer.


So it was proceeded with preparing eletrolyte with the following composition :
200g/l ammonium nitrate
40ml/l 68% nitric acid
*surfactant (dish soap) in trace amount was added to supress possible lead bearing spray during elecrodeposition stage and form a stable foam instead.

Electrodes:
1: metallic lead
2: 316 type stainless alloy (abrasively cleaned and pretreated electrolytically to enhance adhesion*)
3: metallic lead


H bridge parameters:

frequency: 2Hz
duty: 3/97 (t1/t2)



DSCF1605.JPG - 1.3MB
Fig.2 The cell with 50ml of electrolyte and the three electrodes suspended in it.



DSCF1607.JPG - 1.1MB
Fig. 3 One can see lead whiskers at the bottom of cell originating from cathodic overdeposition of lead during t1 period.




DSCF1608.JPG - 1.1MB
Fig.4 A more generic view of the setup (I apologize for the crude setting)

The deposition process was continued for 30 minutes under room temperature (21C) and at the aforementioned parameters. The electrodeposition of lead dioxide at the central stainless substrate electrode started as different colored batches and stripes on the surface and the proceeded to take on a dark, almost black glossy appearance over the entire submersed surface area of the central electrode surface. Gas evolution on central electrode was minimal, but more pronounced during the first minutes and died down after that to only some bubbles sticking to electrode surface. These were removed periodically, by lifting the electrode out of the cell momentarily and submersing it back in.



DSCF1612.JPG - 871kB
DSCF1614.JPG - 785kB
DSCF1613.JPG - 808kB

Fig. 5 The resulting lead dioxide layer on the central stainless substrate after 30min of deposition time


The resultant layer is of a bluish black coloration, has a glossy appearance and seems to be well adhered. At least visually what one could classify as a most impressive result.

Closer observation under a USB microscope reveals that the sample is quite uniformly coated and seems intact.



USB 2.0 Camera-3.18-15;26;49;285.jpg - 327kB

USB 2.0 Camera-3.18-15;28;50;36.jpg - 337kB

USB 2.0 Camera-3.18-15;27;43;285.jpg - 375kB
Fig. 6 The coating as seen under magnification of USB microscope



[Edited on 18-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 20-3-2018 at 04:10



Here one can observe the results of a "thicker" coating of presumably beta PbO2 that failed to adhere to substrate due to internal stresses that develop during the layer formation process.

The layer was formed via the method described in previous post, but the plating conditions were altered as following:

t1/t2: 2/98
frequency: 10Hz
plating duration: 120min
current density: around 3mA/cm2

USB 2.0 Camera-3.20-14;0;7;399.jpg - 227kB

The higher freqency seems to allow for a thicker coating of PbO2 to form without stress cracking.
The coats formed at 2Hz frequency were subject to stress cracking only after 40min of electrodeposition vs. the same occuring at about 120min plating duration at 10Hz.




Exact science is a figment of imagination.......
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6467
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 20-3-2018 at 04:25


Surprised no one has commented yet markx. This is impressive work. If they test out ok under use then this is worthy of prepub. That finish looks really tidy.



View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 8149
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 20-3-2018 at 04:46


At first when I read about this, I was thinking in the lines of "a difficult way to get some PbO2 on an electrode", but this setup actually really is smart :)

I myself have thought about similar things, but I always ended up with a 2-stage process. First taking a lead anode and a cathode of any material, and pushing a lot of current through this, making the anode dissolve. You always lose some lead though on the cathode again. The second step then is replacing the cathode by a fresh piece of material and using that as anode. That's a lot of plugging and hard to control.

In this setup you will finally get a certain fairly stable Pb(2+) concentration and deposition of lead on the cathode (rightmost electrode) and deposition of PbO2 on the center electrode.

I am looking forward to see how the electrodes, made in this process, perform when used for electrolysis. If you can make some perchlorate from chlorate with this setup, then that would be really interesting. Perchlorates are quite hard to make electrolytically and using the chlorate melting method is quite risky, with risk of explosion or uncontrolled runaway and foaming of molten KClO3/KClO4. So, any progress in this direction is welcome.




The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 20-3-2018 at 04:57


Quote: Originally posted by j_sum1  
Surprised no one has commented yet markx. This is impressive work. If they test out ok under use then this is worthy of prepub. That finish looks really tidy.


Thanks for the kind words! :)
It is a really facinating subject and has been haunting me for the longest time....there seems to be great potential in this approach and I try to follow it to the extent that my abilities and resources allow me to.
To be honest, the current substrate material is not really the best option to choose for a functional and durable anode in agressive electrosynthesis conditions (halide bearing solutions e.g.), but it allows me to study the effect of the parameters related to the "novel" electrodeposition process and that in itself is quite satisfactory at the time.
I did test the small anodes in an improvised perchlorate cell containing relatively pure (carefully recristallised) KClO3 solution as the electrolyte and to my amazement they held up for several hours of torture before I could see the iron starting to slowly dissolve from beneath the areas of most current density and dicoluring the solution slightly yellow. The coating itself remained intact (did not discolor, deform or peel off in the cell). But after removing the anode from perchlorate cell, flushing with water and wiping with a paper towel, the coating broke partly off in the most afftected areas: corners, edges. A rather predictable outcome as the stainless steel corroded beneath the oxide and broke the adhesive bond.
In defence of this awaited failure I must say that these coatings used in the perchlorate cell were really thin: deposited during 15 and 30 min of plating time in the lead cell and despite their fragile nature they still managed to hold up for far longer than I could have predicted.
A proper thicker coating will no doubt resist for far longer and perhaps even yield a working anode on a stainless substrate (now that would be outstanding)....although I would preferably switch to titanium once the optimum plating conditions are worked out. This of course creates another obstacle regarding the passivation blocking layer that need to be applied on a Ti substrate before PbO2 coating can be deposited, but prior art exists and we all love a good challenge :)




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 24-3-2018 at 13:11



Here one can observe the formation of PbO2 forming through different colored deposit layers on the verge of the electrolyte contact point with the stainless substrate:

USB 2.0 Camera-3.24-22;58;38;116.jpg - 209kB

USB 2.0 Camera-3.24-23;3;18;96.jpg - 263kB

The upper part is the uncoated stainless substrate and lower part is unifrom layer of PbO2 formed on it at following conditions:

t1/t2: 2/98
frequency: 10Hz
deposition time: 60min
@ 21C electrolyte temperature



DSCF1616.JPG - 908kB DSCF1620.JPG - 842kB

[Edited on 24-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 26-3-2018 at 05:44



The sample from last post happily bubbling away in a small perchlorate cell (KClO3 solution):

DSCF1623.JPG - 983kB

DSCF1621.JPG - 1023kB

DSCF1625.JPG - 912kB

Unfortunately the coating is not perfect enough to shield the substrate metal and it starts to corrode after about two hours of operation.

Titanum still seems to be the only viable option for a durable anode of this type.

This brings me to the aforementioned obstacle regarding choices of passivation prevention coating for titanium....I guess the tin oxide option is one of the most doable routes? Does anyone have any other reasonably simple options to suggest for this purpose?

I guess manganese oxide could also be one of the things to try....




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 26-3-2018 at 08:42


The result of trying to deposit PbO2 on a mechanically cleaned Ti substrate without an intermediate layer to counteract passivation:

USB 2.0 Camera-3.26-19;34;29;607.jpg - 258kB

As can be seen the deposition is uneven and takes place on only the centers that passivated slow enough to allow for a conductive PbO2 layer to form before the current flow ceased.

t1/t2: 2/98
frequency: 10Hz
deposition time: 35min
current density: unknown due to the passivated surface
electrolyte temperature: 21C

The blotchy layer is strongly adhered and can not be wiped off the surface.



You know what the weirdest part is.....this abomination actually conducts:


DSCF1634.JPG - 938kB DSCF1644.JPG - 1MB

Going to see for how long though....

[Edited on 26-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 26-3-2018 at 11:43


As could be expected the Ti substrate anode is passivating at a rather progressive rate....

The initial current through the perchlorate cell was around 10mA

at 60min the current was 7mA
at 100min the current was 4,5mA
at 170min the current was 2mA

I project that around 200min the anode shall be passivated permanently....

[Edited on 26-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 26-3-2018 at 12:04



Yup.....I see a dead anode :D

USB 2.0 Camera-3.26-22;57;44;879.jpg - 292kB

By 190min the current has fallen below 1mA and gas evolution has practically stopped on the surface.

The PbO2 layer looks quite identical to what it was in the beginning, but clearly the titanium substrate has passivated to a point where current can no longer pass to the lead dioxide deposit.






Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 26-3-2018 at 16:20


Here one can observe another interesting sample of lead dioxide deposition on "bare" Ti substrate:

USB 2.0 Camera-3.27-1;56;23;668.jpg - 261kB

In this case I thoroughly sanded the lower edge of a Ti strip to clean metal and left the upper part as it was....under a deposit of years worth of oxide. It was immediately placed into the PbO2 deposition bath under the same conditions as before:

t1/t2: 2/98
frequency: 10Hz
deposition time: 30min
electrolyte temperature: 21C

What is interesting is that most of the deposition centers occur in the pitting of the uncleaned and presumably thoroughly passivated upper part of the strip and the abrasively cleaned lower part of Ti is virtually void of any deposit.
I find that highly intriguing.....does the titanium oxide layer under some favorable conditions create a preferred site for the deposition of lead dioxide?

I also cleaned another strip of the same Ti stock thoroghly by sanding it completely to bare metal and placed it into the lead dioxide bath for 30min....virtually no deposition occurred on the surface.




Now look at the sample below:

USB 2.0 Camera-3.27-2;37;20;339.jpg - 255kB


USB 2.0 Camera-3.27-2;41;10;658.jpg - 194kB

In an attempt to create a slightly oxidised surface favoring deposition, I thoroughly sanded this sample to bare metal and then electrochemically etched it in ammonium heptamolybdate solution (30g/l) in alternating current mode of 50% anodic duty and 5Hz frequency for 20 min.
During that treatment the titanium first showed signs of passivation coloring, which appeared as different colored stripes of red, green and brown on the surface. After about 5 minutes the surface of Ti turned a matte black and remained as such for the whole duration of the treatment. The black layer was not adherent and could be wiped/washed off with some effort, revealing an ever so slightly beige colored surface.
In such state it was placed into the lead dioxide bath under the same conditions as previous Ti sample and at first it seemed to be passivated. After 10min it was apparent that deposition of PbO2 is taking place quite evenly over the entire submersed surface of the sample. There was an obvious abundance of initial deposition centers compared to previous samples. The initially even deposition then progressed into an uneven one, favoring some regions of the substrate, but still it was more uniform than in previous attempts. After 2 hours of deposition I ended up with the sample that can be seen in the last pictures.




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 29-3-2018 at 12:04


Status update:

For practical purposes it seems I have solved at least the problem of creating a passivation blocking intermediate layer on Ti.


DSCF1662.JPG - 894kB
Fig. 1 Take a piece of raw Ti with desired dimensions and sand clean to expose bare metal surface


DSCF1663.JPG - 1.1MB
Fig. 2 Acquire chloroplatinic acid solution from convenient sources.


DSCF1664.JPG - 982kB
Fig. 3 Cover Ti substrate with chloroplatinic acid solution and heat carefully to 300-400C, obtain Pt clad titanium substrate.


DSCF1666.JPG - 925kB
Fig. 5 Plate over with PbO2 at preferred conditions.


DSCF1668.JPG - 1.1MB
Fig. 6 Subject the anodes to torture in perchlorate cell conditions.





Exact science is a figment of imagination.......
View user's profile View All Posts By User
j_sum1
Administrator
********




Posts: 6467
Registered: 4-10-2014
Location: At home
Member Is Offline

Mood: Most of the ducks are in a row

[*] posted on 29-3-2018 at 13:06


Markx, I think you have made stunning progress here.
It would be great if you could write up the full procedure including electronics and put it in prepub.




View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 30-3-2018 at 12:25


Quote: Originally posted by j_sum1  
Markx, I think you have made stunning progress here.
It would be great if you could write up the full procedure including electronics and put it in prepub.


I'm honored by the proposal :)

But I would like to first work out a more or less working solution for this topic and then proceed to summarizing it in a compact form....


As far as current experimentation shows the PbO2 coatings deposited by the bath composition that I have used so far are not stable in the perchlorate cell conditions. The coatings tend to deform and flake off from the surface of the anode.



USB 2.0 Camera-3.28-0;1;48;467.jpg - 137kB
Fig. 1 Initial coating on Pt clad Ti substrate (60min deposition at 10Hz)



USB 2.0 Camera-3.29-21;44;28;154.jpg - 177kB USB 2.0 Camera-3.29-21;45;4;541.jpg - 190kB
Fig. 2 Same coating after 30h in perchlorate cell conditions (facing away from cathode vs. facing to cathode respectively from left to right)

As one can clearly see the PbO2 coating is completely flaked off and rendered ineffective. The Pt clad substrate is still conductive and shows no signs of passivation, which is a great succes in its own so far.
What is even better....the substrate can be chemically etched clean and reused to deposit a new coating.

To achieve that one has to immerse it into solution of citric acid+ammonium citrate+ acorbic acid for a few minutes. The proportions are not critical and all of the PbO2 remnants shall be dissolved completely leaving the substrate unharmed and ready dor a new coating.


To combat the internal stresses and flaking of the coatings I decided to modify the deposition bath composition by adding 1g/l of Silipon RN 31 (sodium lauryl sulfate). This seems to have reduced the deposition rate of the PbO2, at least by visual assessment, but allows to deposit a uniform and much thicker coating without developing stress cracking.




USB 2.0 Camera-3.30-21;22;30;114.jpg - 90kB USB 2.0 Camera-3.30-22;28;27;784.jpg - 92kB USB 2.0 Camera-3.30-22;28;58;440.jpg - 93kB
Fig. 3 Deposits on Pt clad Ti substrate from the Silipon modified bath at 60/120/180 min deposition time at 10Hz from left to right respecitvely

As can be seen the deposit is of a matte apperance as opposed to shiny and looks totally uniform without any stress cracking or other defects across the entire surface. Pervious bath composition allowed for a maximum of 120 minutes of deposition before stress cracks appeared on the surfave of coatings.

I also measured the deposition rate by weighing the sample after every hour ant the rate was pretty much constant at 20mg/h. Quite low, but if it allows to build a stress free thick coating, then it might be the way to a durable anode.


USB 2.0 Camera-3.30-23;37;48;714.jpg - 95kB
Fig. 4 Deposit at 240 minutes....still totally uniform and no cracking or defects (deposition rate holds constant at 20mg/h)

The white fibres that can be seen on surface originate from paper towel I use to dry the deposit after removing from deposition bath. They get snagged on suface and can not be removed completly....also they seem to codeposit as can be seen on last image :)



[Edited on 30-3-2018 by markx]




Exact science is a figment of imagination.......
View user's profile View All Posts By User
markx
National Hazard
****




Posts: 657
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline

Mood: Very Jolly

[*] posted on 30-3-2018 at 13:53


The coating at 300 minutes. The corner broke off because I dropped it onto the floor :D Makes a great illustration of the thickness though...

USB 2.0 Camera-3.31-0;44;10;142.jpg - 91kB

USB 2.0 Camera-3.31-0;48;6;347.jpg - 47kB




Exact science is a figment of imagination.......
View user's profile View All Posts By User
 Pages:  1  ..  40    42    44  ..  47

  Go To Top