Author: Subject: Perchlorate cell cathode
Chemgineer
Hazard to Others
***




Posts: 223
Registered: 25-5-2021
Member Is Offline


[*] posted on 22-5-2023 at 13:24
Perchlorate cell cathode


I have been running a sodium perchlorate cell with a PbO2 anode and a Ti mesh cathode, One thing that keeps happening is the cathode gradually bends and curves away from the anode.

This doesn't happen with my chlorate cell with MMO and Ti.

Has anyone else had this happen?
View user's profile View All Posts By User
Rainwater
National Hazard
****




Posts: 989
Registered: 22-12-2021
Member Is Offline

Mood: Break'n glass & kick'n a's

[*] posted on 22-5-2023 at 13:34


When I was testing reaction conditions, using 22awg titanium wire coated in PbO and high current I noticed this, figured it was a thermal expansion effect, like with a bi metal strip



"You can't do that" - challenge accepted
View user's profile View All Posts By User
yobbo II
National Hazard
****




Posts: 773
Registered: 28-3-2016
Member Is Offline

Mood: No Mood

[*] posted on 23-5-2023 at 07:18



I think its hydrogen absorption on one side more that the other.
View user's profile View All Posts By User
Chemgineer
Hazard to Others
***




Posts: 223
Registered: 25-5-2021
Member Is Offline


[*] posted on 23-5-2023 at 07:56


Quote: Originally posted by yobbo II  

I think its hydrogen absorption on one side more that the other.


That could be right because eventually the cathode fails and it might be because of hydrogen embrittlement.
View user's profile View All Posts By User
mysteriusbhoice
Hazard to Others
***




Posts: 477
Registered: 27-1-2016
Member Is Offline

Mood: Became chemistry catboy Vtuber Nyaa

[*] posted on 23-5-2023 at 12:09


Quote: Originally posted by Chemgineer  
I have been running a sodium perchlorate cell with a PbO2 anode and a Ti mesh cathode, One thing that keeps happening is the cathode gradually bends and curves away from the anode.

This doesn't happen with my chlorate cell with MMO and Ti.

Has anyone else had this happen?

I actually want to know how to get a Ti mesh to become like this because they make for a very good substrate.
Anyways this is why i've stopped using Ti cathodes apart from it's terrible H2 evolution potential causing it to reduce the electrolyte lowering efficiency.
Use a copper or nickel cathode for perchlorate cells as it's much better. Lead cathode is even worse than Ti has highest H2EP. Steel is decent if nickel plated or carbon steel.