Sciencemadness Discussion Board
Not logged in [Login ]
Go To Bottom

Printable Version  
Author: Subject: Covering Fluxes
redmoon
Harmless
*




Posts: 2
Registered: 7-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 8-12-2010 at 03:09
Covering Fluxes


Hi everyone,

I need a covering flux that has a low melting point such as 200 celcius degree or less. A salt flux may be helpfull. I am looking forward your advices.

Thanks :)
View user's profile View All Posts By User
not_important
International Hazard
*****




Posts: 3873
Registered: 21-7-2006
Member Is Offline

Mood: No Mood

[*] posted on 8-12-2010 at 09:41


What is it covering? Most low MP salt mixes as based on alkali metal nitrates or hydroxides, both of which are likely to react with many metals.

At the temperature you want I suspect you'll hae to go with organics, even just plain oil.

View user's profile View All Posts By User
redmoon
Harmless
*




Posts: 2
Registered: 7-12-2010
Member Is Offline

Mood: No Mood

[*] posted on 18-12-2010 at 05:11


i need flux to cover lead metal
View user's profile View All Posts By User
Magpie
lab constructor
*****




Posts: 5939
Registered: 1-11-2003
Location: USA
Member Is Offline

Mood: Chemistry: the subtle science.

[*] posted on 18-12-2010 at 08:19


I have done fire assays on gold ore having a quartz matrix. For this assay PbO is reduced to lead which collects as a button at the bottom of the crucible. IIRC my furnace temperature was in the vicinity of 800-900C. I used a salt (NaCl) cover as recommended by Ammen in his book "Recovery and Refining of Precious Metals." Ammen also cites the use of borax as a cover.

melting points:

Pb................327C
NaCl.............800C
Na2B4O7.....741C

Is this relevant to what you are trying to do?

[Edited on 18-12-2010 by Magpie]




The single most important condition for a successful synthesis is good mixing - Nicodem
View user's profile View All Posts By User
watson.fawkes
International Hazard
*****




Posts: 2793
Registered: 16-8-2008
Member Is Offline

Mood: No Mood

[*] posted on 18-12-2010 at 08:34


Quote: Originally posted by redmoon  
i need flux to cover lead metal
If it's chemically compatible with what you're doing, you could use refined bitumen, used commercially as roofing tar and for asphalt roadbed repairs.
View user's profile View All Posts By User

  Go To Top