Author: Subject: testing a round bottom flask
itsafineday
Hazard to Self
**




Posts: 89
Registered: 5-1-2019
Location: "...in them thar hills."
Member Is Offline

Mood: Feelin groovy

[*] posted on 19-1-2019 at 05:36
testing a round bottom flask


I received a couple of round bottom flasks from china and they have some warps and flat spots in them. I mentioned my concerns to the supplier and they said to test them and they would replace them if they broke.

I have a pump and hotplate but don't really know how to test these without risking destroying equipment. Any suggestions?
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3738
Registered: 8-2-2015
Location: 3rd rock from the sun
Member Is Offline


[*] posted on 19-1-2019 at 08:45


Can you post one or more photographs ?



CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
XeonTheMGPony
International Hazard
*****




Posts: 1641
Registered: 5-1-2016
Member Is Offline

Mood: No Mood

[*] posted on 19-1-2019 at 08:56


to test:

Dry heat it, to 200c, allow to cool
Dry heat hot to touch, add room temp distilled water
Boil water then place in cool water bath (10c apx)
Dry heat again

If it survives that it should survive the bulk of lab use.
View user's profile View All Posts By User
Metacelsus
International Hazard
*****




Posts: 2542
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline

Mood: Double, double, toil and trouble

[*] posted on 19-1-2019 at 10:33


You might also want to test pulling a vacuum on them. If you have a polarizing filter you can also look for stress points within the glass.



As below, so above.

My blog: https://denovo.substack.com
View user's profile View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 19-1-2019 at 11:42


modification of xeon's tests.

Heat in oven to maximum temperature (most ovens this will be somewhere near or over 200c.)
Allow to cool to room temperature.
Place the flask in a pan of boiling water (borosilicate glass should withstand 160C temp change)
Allow the flask to sit in boiling water until it is hot then place in a mix of ice and water (0C).
Next pull a full vacuum on the flask.

The last dry heat is probably redundant.
View user's profile View All Posts By User
XeonTheMGPony
International Hazard
*****




Posts: 1641
Registered: 5-1-2016
Member Is Offline

Mood: No Mood

[*] posted on 19-1-2019 at 14:31


Why I do the final dry heat is one to dry it, but two is to show any fissures that may have formed, so for me it is the final pass n dry befor it goes into the shelf
View user's profile View All Posts By User
itsafineday
Hazard to Self
**




Posts: 89
Registered: 5-1-2019
Location: "...in them thar hills."
Member Is Offline

Mood: Feelin groovy

[*] posted on 19-1-2019 at 16:23


Awesome replies! Thank you VERY much. This will be fun and if they survive I should have more confidence in them than if they were perfects. Really, one just has a little divot but the other is 4 grams lighter and has a fairly large sag. The supplier is always super cool about issues but they will certainly let me keep crap if I don't catch it.

I'm not a smartphone user so posting a pic means borrowing a camera.
View user's profile View All Posts By User
VSEPR_VOID
National Hazard
****




Posts: 719
Registered: 1-9-2017
Member Is Offline

Mood: Fullerenes

[*] posted on 19-1-2019 at 17:48


Wrap your hot plate's top in foil to keep it clean if something breaks. Also make sure to store your electronic equipment, such as hotplates, in a low humidity environment and keep them clean.



Within cells interlinked
Within cells interlinked
Within cells interlinked
View user's profile View All Posts By User
itsafineday
Hazard to Self
**




Posts: 89
Registered: 5-1-2019
Location: "...in them thar hills."
Member Is Offline

Mood: Feelin groovy

[*] posted on 20-1-2019 at 09:03


Quote: Originally posted by Metacelsus  
You might also want to test pulling a vacuum on them. If you have a polarizing filter you can also look for stress points within the glass.


Is a polarizing filter like a polarized lens ? What do the stress points look like?
View user's profile View All Posts By User
itsafineday
Hazard to Self
**




Posts: 89
Registered: 5-1-2019
Location: "...in them thar hills."
Member Is Offline

Mood: Feelin groovy

[*] posted on 20-1-2019 at 11:48


So one of the 500ml flasks went from 170c to 32 c and went crackle but didn't fall apart. The other 500ml handled 150 c to 32c without a problem. The ball canning jar I threw into the mix because I just had to know and it cracked and fell apart when it went from 140 to 32c . All three were able to take going from boiling water to ice water without issue.
View user's profile View All Posts By User
macckone
Dispenser of practical lab wisdom
*****




Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline

Mood: Electrical

[*] posted on 26-1-2019 at 22:44


To achieve the full 160C, the glass has to be pretty close to perfect.
Boiling water to ice water is only 100C and usually more than sufficient for everyday lab work.
Ball canning jars are not designed to go from boiling to ice, I am really surprised that survived.
What did you use for 32C? are you sure you don't mean 0C (32F)?
View user's profile View All Posts By User
itsafineday
Hazard to Self
**




Posts: 89
Registered: 5-1-2019
Location: "...in them thar hills."
Member Is Offline

Mood: Feelin groovy

[*] posted on 27-1-2019 at 05:09


I was using an infrared thermometer . I did the boiling water to ice water test first. The ice water was left on the stove as the oven heated over 30 minutes so the ice in the water melted and apparently the water warmed a bit. I was pretty shocked about the mason jar , too. Ball mason jars kick butt. The one flask actually survived the dry heat of 140c and the 32 c water quench. I don't know how accurate one of these thermometers is for something like an empty rbf, though.

So , to be honest, I think I was a bit unfair in the test with the oven. I was glad that I was able to piggy back the rbf with another order to minimize the suppliers loss.