[*] posted on 10-6-2007 at 07:15
Electroless Nickel Plating


[This topic seem suited for this forum since it's halfway trough electroplating]

Has anybody ever heard of electroless nickel plating? What is the composition of the solution? All I can find is that it's a Nickel/Phosphorous alloy, but no in detail compostion of the solution. Anybody has any info/paper on that?




/}/_//|//) /-\\/|//¬/=/_
My PGP Key Fingerprint: D4EA A609 55E4 7ADD 8529 359D D6E2 33F6 4C76 78ED
View user's profile View All Posts By User This user has MSN Messenger
solo
International Hazard
*****




Posts: 3973
Registered: 9-12-2002
Location: Estados Unidos de La Republica Mexicana
Member Is Offline

Mood: ....getting old and drowning in a sea of knowledge

[*] posted on 10-6-2007 at 07:28


Here are a few references to assist you....solo

ftp://electrochem.cwru.edu/pub/estir/proc.txt
http://www.corrosion-doctors.org/MetalCoatings/Electroless.h...
http://electrochem.cwru.edu/estir/proc.htm#dtop
ftp://electrochem.cwru.edu/pub/estir/

[Edited on 10-6-2007 by solo]




It's better to die on your feet, than live on your knees....Emiliano Zapata.
View user's profile View All Posts By User
Blind Angel
National Hazard
****




Posts: 845
Registered: 24-11-2002
Location: Québec
Member Is Offline

Mood: Meh!

[*] posted on 10-6-2007 at 07:46


I gratefully thank you for the linké

Electroless nickel plating (From a Meeting of the American Society for Testing and Materials, ASTM Special Technical Publication No. 265)
ASTM, Philadelphia, PA 1959.
and
Electroless deposition of metals and alloys (From the 172nd Meeting of The Electrochemical Society, Honolulu, Oct. 1987, ECS Proceedings, Vol. 88-12)
M. Paunovic and I. Ohno (Ed), ECS, Pennington, NJ 1988.
would be interesting, the other are either redundant or only say: electroless is good for you, find somebody to do it.




/}/_//|//) /-\\/|//¬/=/_
My PGP Key Fingerprint: D4EA A609 55E4 7ADD 8529 359D D6E2 33F6 4C76 78ED
View user's profile View All Posts By User This user has MSN Messenger
solo
International Hazard
*****




Posts: 3973
Registered: 9-12-2002
Location: Estados Unidos de La Republica Mexicana
Member Is Offline

Mood: ....getting old and drowning in a sea of knowledge

[*] posted on 10-6-2007 at 07:58


Composition of solution information........solo

http://www.alu-info.dk/HTML/alulib/modul/A00364.htm




It's better to die on your feet, than live on your knees....Emiliano Zapata.
View user's profile View All Posts By User
woelen
Super Administrator
*********




Posts: 7988
Registered: 20-8-2005
Location: Netherlands
Member Is Offline

Mood: interested

[*] posted on 10-6-2007 at 11:21


Be careful with the sodium hypophosphite. In many countries in the world this is a so-called list I chemical, and as such it is highly watched and suspect. Sodium phosphite in fact is quite benign and not dangerous at all, but apparently it is an important precursor for meth-cooks and that's why it is so suspect. This makes me mad :mad:.



The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
Tacho
National Hazard
****




Posts: 582
Registered: 5-12-2003
Member Is Offline

Mood: No Mood

[*] posted on 11-6-2007 at 13:37


This is a very comprehensive text on electroless nickel:

http://www.ias.ac.in/sadhana/Pdf2003JunAug/Pe1104.pdf

I once obtained some plating using magnesium hypophosphite instead of sodium hyphosphite.

Hope this helps.