calcium nitrite synthesis


i am trying to synthesis calcium nitrite.
i have taken calcium nitrate and tried to reduce it to calcium nitrite by using a reducing agent and also by thermal treatment. but i m not getting the desired product .
how about using ammonium nitrate and lime? or using sodium nitrite and lime?
is there any other way to synthesis calcium nitrite...please let me know

[Edited on 5-9-2003 by karandikarmv]
View user's profile View All Posts By User
Mephisto
Chemicus Diabolicus
***




Posts: 295
Registered: 24-8-2002
Location: Germany
Member Is Offline

Mood: swinging

[*] posted on 5-9-2003 at 01:54


I know for sure, that there is a synthesis described in the first volume of the second edition of „Handbook of Preparative Inorganic Chemistry“ (G. Brauer, Academic Press, New York, 1963). It’s a standard reference work, so you can find it in the most libraries.

Reduction of calcium nitrate with lead didn’t work?
View user's profile Visit user's homepage View All Posts By User
karandikarmv
Harmless
*




Posts: 6
Registered: 4-9-2003
Location: india
Member Is Offline

Mood: very depressed

[*] posted on 8-9-2003 at 00:15


Mephisto
i have checked in the book, but its not there
View user's profile View All Posts By User
Mephisto
Chemicus Diabolicus
***




Posts: 295
Registered: 24-8-2002
Location: Germany
Member Is Offline

Mood: swinging

sad.gif posted on 8-9-2003 at 08:52


Sorry, I checked it too fast. So I messed up calcium nitrite with calcium nitride.



Maybe you’ve got an other process, which evolves nitrous fumes. You can lead the fumes through Ca(OH)2 and get a solution of calcium nitrite. A nice way of recycling.

Sorry for the misguidance.:(
View user's profile Visit user's homepage View All Posts By User
karandikarmv
Harmless
*




Posts: 6
Registered: 4-9-2003
Location: india
Member Is Offline

Mood: very depressed

[*] posted on 8-9-2003 at 20:10


Mephisto

is the following reaction possible?
Ca(NO3)2------ Ca(NO2)2 +O2
what is the temp. at which O2 will be evolved from Ca. nitrate?
the manufactures of Ca-nitrite claim it to be 500 deg.C
i have tried the above reaction and could get some Ca.nitrite, analysed as NO2 by spectro. method, but its only ~20% conversion from nitrate to nitrite.
does recrystallisation required?
i am interested in 100%conversion of nitrate to nitrite.
i have also searched literature on the net and in library,but unable to get a complete paper.
View user's profile View All Posts By User
Mephisto
Chemicus Diabolicus
***




Posts: 295
Registered: 24-8-2002
Location: Germany
Member Is Offline

Mood: swinging

[*] posted on 9-9-2003 at 08:37


There isn’t much source material about the synthesis of calcium nitrite. The conversion of calcium nitrate to the nitrite won’t work. Here’s what I found:

‚Calcium nitrite decomposes to calcium oxide and a mixture of nitrogen monoxide and nitrogen dioxide at temperatures as low as 250 °C.‘ That’s the reason why calcium nitrate is directly converted to calcium oxide. ‚Thermal decomposition of calcium nitrate begins at 500 °C.
Ca(NO3)2 --> CaO + 2 NO2+ 1/2 O2 DH = +369 kJ/mol‘

A recrystallistion is possible, but I haven’t the exact solubility data. Only that:

‚The nitrite can be recovered as the tetrahydrate Ca(NO2)2 · 4H2O by concentration and cooling. This product has a lower solubility than calcium nitrate tetrahydrate Ca(NO2)2· 4H2O.‘

The synthesis form Ca(OH)2 and nitrous gases yields to a technical product:

‚Calcium nitrite is formed when a mixture of gaseous nitrogen dioxide and nitrogen monoxide (OD < 50 %) is absorbed in a suspension of calcium hydroxide. This process is used to clean up the final tail gases from low-pressure nitric acid plants when no demand exists for sodium nitrate or sodium nitrite. The spent absorption liquor contains calcium nitrite and generally some calcium nitrate.‘

I hope, I could help a little bit. If you get access to a Beilstein database, you should find more.

Quoted from: [Ullmann's Encyclopedia of Industrial Chemistry, Sixth Edition, 2002 Electronic Release (c) Wiley-VCH. Weinheim. Germany.]

[Edited on 9-9-2003 by Mephisto]
View user's profile Visit user's homepage View All Posts By User
madscientist
National Hazard
****




Posts: 962
Registered: 19-5-2002
Location: American Midwest
Member Is Offline

Mood: pyrophoric

[*] posted on 11-9-2003 at 12:21


http://www.sciencemadness.org/talk/viewthread.php?tid=52



I weep at the sight of flaming acetic anhydride.
View user's profile View All Posts By User
karandikarmv
Harmless
*




Posts: 6
Registered: 4-9-2003
Location: india
Member Is Offline

Mood: very depressed

[*] posted on 17-9-2003 at 21:37


Mephisto

today i got a little success,i hope that i have got some ca- nitrite, i am trying to analyse the nitrite in calcium nitrite

the spectrophotometric method for nitrite is only for low concentration of nitrite... so i am trying the volumetric method as per ASTM using potassium permanganate and sodium oxalate

do u suggest any other method for high nitrite concentration?
View user's profile View All Posts By User
Mephisto
Chemicus Diabolicus
***




Posts: 295
Registered: 24-8-2002
Location: Germany
Member Is Offline

Mood: swinging

[*] posted on 18-9-2003 at 03:35


Sorry, I haven’t much knowledge about volumetric analysis.

BTW, why are intersted in another method? The KMnO4 and oxalate method should be right.
View user's profile Visit user's homepage View All Posts By User
kingspaz
Hazard to Self
**




Posts: 55
Registered: 23-7-2002
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 18-9-2003 at 06:26


would it not be possible to convert by recrystalisation?

like make some KNO2. make a hot saturated solution of Ca(NO3)2 and the KNO2 then allow to cool....KNO3 will crystalise out (i think, i have no solubility data to hand a bad memory!) then you're left with Ca(NO2)2 in solution.




the unexamined life is not worth living to a human
View user's profile View All Posts By User
Sedit
International Hazard
*****




Posts: 1939
Registered: 23-11-2008
Member Is Offline

Mood: Manic Expressive

[*] posted on 15-3-2009 at 13:06


[moved]

[Edited on 16-3-2009 by Sedit]





Knowledge is useless to useless people...

"I see a lot of patterns in our behavior as a nation that parallel a lot of other historical processes. The fall of Rome, the fall of Germany — the fall of the ruling country, the people who think they can do whatever they want without anybody else's consent. I've seen this story before."~Maynard James Keenan
View user's profile View All Posts By User
Rosco Bodine
Banned





Posts: 6370
Registered: 29-9-2004
Member Is Offline

Mood: analytical

biggrin.gif posted on 16-9-2010 at 09:10
Calcium Nitrite from Sodium Nitrite and Hydrated Lime


Quote: Originally posted by karandikarmv  
i am trying to synthesis calcium nitrite.
i have taken calcium nitrate and tried to reduce it to calcium nitrite by using a reducing agent and also by thermal treatment. but i m not getting the desired product .
how about using ammonium nitrate and lime? or using sodium nitrite and lime?
is there any other way to synthesis calcium nitrite...please let me know

[Edited on 5-9-2003 by karandikarmv]


Hopefully nobody was in a big hurry for an answer to your question :D

Sodium Nitrite and Lime will work . See attached patent US4294813

Attachment: US4294813 Calcium Nitrite from Sodium Nitrite.pdf (103kB)