I only nitrated it for 1 hour, so I know it won't be quite as energetic as some that have nitrated for longer. It burned suprisingly well, but it did take a while for it to burn completely down, which is kind of unlike nitrocellulose. It had a flame that kind of looked like when you burn ethanol. In all it took about 10 seconds for it to burn completely.


Attachment: phpUFJ0YK (394kB)
This file has been downloaded 46 times

Attachment: php1qjqOU (394kB)
This file has been downloaded 42 times

Attachment: phpH34Yqy (394kB)
This file has been downloaded 39 times

View user's profile View All Posts By User
Maui3
Hazard to Self
**




Posts: 71
Registered: 9-9-2024
Member Is Online


[*] posted on 30-10-2024 at 06:00


https://imgur.com/a/B6sJi4d
View user's profile View All Posts By User
bnull
Hazard to Others
***




Posts: 484
Registered: 15-1-2024
Location: South of the border, wherever the border is.
Member Is Offline

Mood: Happy New Year!

[*] posted on 30-10-2024 at 08:17


It looks like common cotton to me; it was probably only slightly nitrated. Did you test your products? Nitrocellulose is soluble in (1) ether:ethanol and (2) acetone. Put a piece of the supposed nitrocellulose together with one of the solvents in a test tube, leave it alone for a while, then transfer the liquid to a glass dish or plate. If there is nitrocellulose, it will form a film--you'll see a residue--in the glass.



Quod scripsi, scripsi.

B. N. Ull

P.S.: Did you know that we have a Library?
View user's profile View All Posts By User
Sir_Gawain
Hazard to Others
***




Posts: 460
Registered: 12-10-2022
Location: [REDACTED]
Member Is Offline

Mood: Stable

[*] posted on 30-10-2024 at 08:55


What are you using to nitrate it?



“Alchemy is trying to turn things yellow; chemistry is trying to avoid things turning yellow.” -Tom deP.
View user's profile Visit user's homepage View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 190
Registered: 12-7-2018
Member Is Offline


[*] posted on 30-10-2024 at 08:56


Guncotton is only in Ethylacetat and Aceton soluble, Celloid is in Alccohol soluble.
Dont use Na2CO3 for neutralisation it can remove the nitrate ions from the cotton only NaHCO3 its not so alkalien. Do nitrate for 2 Hours and under 30C.(mix the acids an day before in an glass container with lid)
If you have Guncotton and you would lithe an ball of this size you would lose your eyes very small pice makes an purpel fireball and you can feel the heat wave. if you have Celloid it burns with and yellow flame and more like an welding flame.
You can it test an an withe ceramic dish if ignited guncotton there is no remains. if you have celloid there are carbon remains (little bit) if your cotton wasnt clean enough there is an yellow spot on the dish.

Maybe your acid mix was to weak 55% nitric acid 1 part on 96% H2SO4 2,8 parts (on mass) or 1 to 2 on Volume. It works i testet it. ps if you add 20% more sulfuric acid doesnt hurt less isnt good. Source: Handbuch der Pulverfabrikation sowie der Schiessbaumwolle und der Schiessheede.

[Edited on 30-10-2024 by Alkoholvergiftung]
View user's profile View All Posts By User
Maui3
Hazard to Self
**




Posts: 71
Registered: 9-9-2024
Member Is Online


[*] posted on 30-10-2024 at 09:13


Bnull, ah should have done that.
Sir_Gawain, I was using 90% Nitric Acid + Conc. Sulfuric Acid.
Alkoholvergiftung, thanks!
View user's profile View All Posts By User
Alkoholvergiftung
Hazard to Others
***




Posts: 190
Registered: 12-7-2018
Member Is Offline


[*] posted on 30-10-2024 at 09:23


If you have acid from 1,42 desteny (concentratet) you need only 1 part nitric on 1,6 part sulfuric acid on Volume or 1 part nitric an 2,16 part H2SO4 on wight.

[Edited on 30-10-2024 by Alkoholvergiftung]
View user's profile View All Posts By User
bnull
Hazard to Others
***




Posts: 484
Registered: 15-1-2024
Location: South of the border, wherever the border is.
Member Is Offline

Mood: Happy New Year!

[*] posted on 30-10-2024 at 09:45


Oops. The solubility of nitrocellulose depends on the degree of nitration. With 8-12% nitrogen, it is called collodion and is soluble in ether:ethanol; with more than 13% nitrogen, it is called guncotton and is insoluble in ether:ethanol. But both collodion and guncotton are soluble in acetone (https://archive.org/details/bigbanghistoryof00brow/page/131/...). Thanks for reminding me of the distinction, @Alkoholvergiftung.