goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
Exact conditionf for preparation of Urushibara nickel
I did not found such thread if i missed such information somewhere sorry for that.
I have read both original papers by Urushibara and monography about this catalyst by Hata.
Procedure for deposition of nickel on zinc to make Urushibara catalyst precursor calls for
mixing 3ml of water with 10g of zinc powder and then adding 10ml solution containing 4.04g NiCl2 * 6H2O (that corresponds to 1g of metallic nickel) on
boiling water bath with string.
One thing seems strange to me: 3ml of water and 10g of zinc powder whatever particle size is it has no chance to be a suspension of zinc in water.
Zinc powder will absorb water.
This procedure is cited on and on and i double checked that i read this correctly.
More over after deposition mixture is filtered on sintered glass funnel so it has to contain significant amount of liquid. Moreover in general
description i read that one should add solution of nickel chloride to suspension of zinc in water.
I would be very grateful for clarification of this. Amount of water is just too low. What is correct amount? About 8 to 9ml of water will form
suspension when mixed with 10g of 80um zinc powder.
Also how long this reaction between zinc and nickel chloride should go?
I read "reaction will soon subside" But soon is 5 seconds or 5 minutes? I should stop it when it will subside but gas will be still evolving or should
i wait until it will completely stop?
Also i did not found any mention about particle size of zinc powder.
I read that somebody here carried out a few experiments with this catalysts and i would be very grateful for any clarification of this. Also any
information (or photos) what i should observe (or not observe) during this reaction will be very helpful.
Also how sensitive to air is U-Ni-B? Can i just pour it from beaker after activation to reaction vessel exposing it to air for a few seconds or should
i protect it from ANY contact with air?
I would like to just to try to reproduce this experiment just for fun and try to reduce some acetone to isopropanol under atmospheric pressure to
check it's activity.
|
|
DavidJR
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 908
Registered: 1-1-2018
Location: Scotland
Member Is Offline
Mood: Tired
|
|
Maybe it's meant to be a paste rather than a suspension. I'm not sure.
Chemplayer did it by tossing nickel chloride solution onto dry zinc dust: https://www.bitchute.com/video/PTSXPBiJvzre/
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
If you want to use it for the reduction, why not use the french pseudo-urushibara, invented many years before Urushibara himself invented these
catalysts?
It is essentially the same, U-Ni-NH3, here is a link: https://www.sciencemadness.org/talk/viewthread.php?tid=20153
I used that method for the amination of ketones, for the reduction of aldehydes, the reduction of oximes and the reduction of an oximinoketone to an
aminoalcohol with huge success.
And you don't even need to form the catalyst separately, it works in-situ.
|
|
goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
@DavidJR: I have seen this video. This procedure is different than original preparation of Urushibara nickel. Lack of stirring, carrying out reaction
at room temperature and lack of showing that prepared catalyst actually exhibits any activity. For this reasons i do not count this video as source of
information.
@karlos³: Thanks for information. I never heard before about this method. Looks very interesting. Are there any references in scientific publication
or only this patent?
I'm happy to read that people from this forum were able to reproduce this but i'm also curious if someone investigated this reaction in greater
detail.
Could You please write two phrases more about conditions that You have used during this reactions?
What should be granulation of zinc powder? Or it is not very important?
Intuition tells me that the finer the better. For example 100um zinc powder will be good enough?
|
|
morganbw
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 561
Registered: 23-11-2014
Member Is Offline
Mood: No Mood
|
|
for the zinc/nickel coupling there is some information/not huge on the hive archives. There is also some information on the vespiary again not huge.
Even though the info of real life use is not huge it is there. Unfortunately mostly not in the forms of scientific papers.
There is enough info for a guideline on how to use. Ignore if you choose, but I feel that the zinc/nickel coupling was/is a gift to an amateur
chemist.
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
It is(a gift for amateur chemist, I mean)!
Just check the zink-nickel thread on there.
I use zinc powder that is sold for fireworks, don't know how fine it is, just the usual stuff.
I use the conditions that were used by Scr0t in the thread on here, in his second experiment.
I achieved 84% yield for the direct amination of phenyl-2-propanone, there is nothing out there thats beat this outcome.
Even phenylacetoxime yielded less product with this reduction.
If you ever want to aminate a ketone to its primary amine, this reaction is your best choice, I really love it.
[Edited on 22-1-2020 by karlos³]
|
|
Abromination
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 432
Registered: 10-7-2018
Location: Alaska
Member Is Offline
Mood: 1,4 tar
|
|
Quote: Originally posted by goldberg ![](images/xpblue/lastpost.gif) | @DavidJR: I have seen this video. This procedure is different than original preparation of Urushibara nickel. Lack of stirring, carrying out reaction
at room temperature and lack of showing that prepared catalyst actually exhibits any activity. For this reasons i do not count this video as source of
information.
@karlos³: Thanks for information. I never heard before about this method. Looks very interesting. Are there any references in scientific publication
or only this patent?
I'm happy to read that people from this forum were able to reproduce this but i'm also curious if someone investigated this reaction in greater
detail.
Could You please write two phrases more about conditions that You have used during this reactions?
What should be granulation of zinc powder? Or it is not very important?
Intuition tells me that the finer the better. For example 100um zinc powder will be good enough? |
I suppose I understand your reasoning in a lack of belief, but chemplayer has proved otherwise to be a very accurate and valuable source to many of
us.
List of materials made by ScienceMadness.org users:
https://docs.google.com/spreadsheets/d/1nmJ8uq-h4IkXPxD5svnT...
--------------------------------
Elements Collected: H, Li, B, C, N, O, Mg, Al, Si, P, S, Fe, Ni, Cu, Zn, Ag, I, Au, Pb, Bi, Am
Last Acquired: B
Next: Na
--------------
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
chemplayer has also attempted the nickel-zinc amination after I suggested that to him: https://twitter.com/ChemPlayer1/status/1124537533394591745
I don't know how it turned out though.
|
|
goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
@karlos³ could You please give me more details about conditions of Your reaction?
especially what was ratio of zinc powder to water. You dissolved 4.04g of NiCl2 * 6H20 in 10ml water or what concentartion you have used? Did You
carried out deposition on boiling water bath or room temperature?
Or You just prepared everything in situ like in mentioned patent?
And did You managed to reduce functional groups that are more resistant than imine or oxime?
@Abromination: I'm just very careful when someone does not tells much about his results like in this video about Urushibara nickel from chemplayer on
youtube.
I'm thinking about good substrate to test. Ideally something that is solid so i could easy do TLC. Sorbic acid? can be cheaply purchased as
preservative and has double bond to hydrogenate. Camphor? Or maybe something like menthol or limonene that i will be able to check by smell?
Also i came across a few papers about deoxygenation of benzyl alcohol and it's deviratives using raney nickel and isopropanol or mixture of ethanol
and water. Does anybody tried this with Urushibara nickel and/or Ni/Zn couple?
Also there is also U-Ni-N activated by just refluxing Ni/Zn in isopropanol. It seems to be even more obscure than U-Ni-A and U-Ni-B. Does anybody
tried to use it?
I'm thinking about good way to examine activity of prepared catalyst. Measurement of absorbed hydrogen will require a little tricky setup especially
to get reasonable precision of measurement..
It would be also interesting to examine mechanism of this reduction i'm open to any suggestions how to do it.
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
I just ran it like in the patent, with the improvements Scr0t mentioned here: http://www.sciencemadness.org/talk/viewthread.php?tid=20153&...
I only reduced an aldehyde to its alcohol, oximinoketones to aminoalcohols, reductively aminated ketones, and reduced oximes to amines.
But the system also reduces double bonds in unsaturated acids, nitriles to amines, and aromatic nitro groups to amines, see here: https://erowid.org/archive/rhodium/chemistry/zn-ni.couple.ht...
However, I haven't tried that, it wasn't interesting to me.
Here is another successful experiment from someone else: https://chemistry.mdma.ch/hiveboard/novel/000470154.html
It is the best system to make primary amines directly from ketones.
If you want to see that in more detail, see the zinc-nickel thread at the vespiary, I have posted all my experiments on there.
I can't access that right now, the site is offline, otherwise I would have posted one of the writeups here.
I dissolve nickel acetate directly in the ammonia solution, add ethanol as cosolvent and the substrate, let it stand a few hours(in case of direct
aminations), and then add three portions of the zinc powder five min apart from each other, with gentle heat in the water bath at the end.
Otherwise you would boil off the ammonia.
[Edited on 23-1-2020 by karlos³]
[Edited on 23-1-2020 by karlos³]
|
|
Corrosive Joeseph
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 915
Registered: 17-5-2015
Location: The Other Place
Member Is Offline
Mood: Cyclic
|
|
Quote: Originally posted by karlos³ ![](images/xpblue/lastpost.gif) |
I only reduced an aldehyde to its alcohol, oximinoketones to aminoalcohols, reductively aminated ketones, and reduced oximes to ketones.
|
Momentary lapse of reason on the last one there..... You reduced oxime to amine.
![;)](./images/smilies/wink.gif)
/CJ
Being well adjusted to a sick society is no measure of one's mental health
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
Oops ![:o](./images/smilies/shocked.gif)
Corrected it.
|
|
Texium
|
Thread Split 23-1-2020 at 19:21 |
goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
How about reduction in basic condition using NiCl2/Zn? Nickel will form hydroxide. I read that reduction of ketones and aldehydes is favored by basic
conditions.
Urushibara has found that nickel on zinc without activation does not exhibit catalytic activity.
So if i'm correctly reasoning hydrogen evolved during precipitation of nickel is used for hydrogenation before insoluble zinc compounds will clog up
catalyst?
Has anybody tried to use external hydrogen source? This route seems very good unless there will be need to acidify post reaction mixture due to
precipitation of zinc hydroxide which will be messy.
Thanks a LOT for information on this but i'm still curious about first precipitation of nickel on zinc and using it as catalyst in separate step.
One pot procedure seems great but it can require quite a bit of zinc powder.
The other problem is that not everything is soluble/misticible with water...
Do You know anything about how pure this zinc has to be? I read that lead is poison for raney nickel. I found one place with zinc powder but it is
contaminated with about 0.1% of lead...
How about making suspension of Urushibara nickel with diluted (say 1%) NaOH or acetic acid, adding compound for hydrogenation and then inserting
cathode (nickel?) electrolytic key (say agar + KCl) and in another beaker anode?
I have found a few papers about raney nickel cathodes and even reduction of pyridine ring in nicotine has been done in quite good yield.
All papers about Urushibara nickel tells for 3ml of water for 10g of zinc (i have checked this again, even paper about study of structure of
Urushibara nickel tells this procedure).
This does not seems like an error. Zinc powder in Japan in 1950s was rather ordinary zinc powder. Is this wrong on purpose?
I have noticed that if there will be 8ml of water of 10g of zinc (this is actually a suspension of zinc in water, not water absorbed on zinc as with
3ml of water) reaction is more vigorous.
I read in Hata monography than the more vigorous reaction the better.
Also does anybody had success with cold prepared Urushibara nickel?
Another thought: how about using colloidal zinc instead of powder? Filtration of used up catalyst will be impossible, the only way will be extraction
of product. But beside that there could be chance for huge surface area right? Unfortunately i did not managed to found any information about
preparation of colloidal zinc.
|
|
stoichiometric_steve
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 827
Registered: 14-12-2005
Member Is Offline
Mood: satyric
|
|
Quote: Originally posted by karlos³ ![](images/xpblue/lastpost.gif) |
the system also reduces double bonds in unsaturated acids, nitriles to amines, and aromatic nitro groups to amines |
Excuse my ignorance, but do you know if this has been tried on nitroalkenes?
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
It has been tried on nitroalkenes, it did not work.
However, it works with the "real" urushibara made from nickel and zinc and digested with formic acid, just not in great yields, as a friend has tried
that.
It is to me of great interest to try it on nitroalkanes sometimes, I am sure it will work very well on them.
|
|
Corrosive Joeseph
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 915
Registered: 17-5-2015
Location: The Other Place
Member Is Offline
Mood: Cyclic
|
|
Please don't write if off just yet...... There was one attempt on nitroalkenes by somebody who had never done the Zn-Ni-NH3 procedure before, it was
not carried out to the letter and no characterization was done.
/CJ
Being well adjusted to a sick society is no measure of one's mental health
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
No, I wrote that off.
He is a good chemist, and that he got absolutely nothing out of it convinces me, that the basic Ni-Zn does not work on nitroalkenes.
However, there is still the acidic urushibara for that, so it does not really matter.
|
|
goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
@karlos³: could You please write here more details about this experiment? Like exact amount of reagents, temperature time and method of isolation and
analysis of products?
Ad reductive amination: is it possible to prepare secondary or trietriary amines with NiCl2 + amine + Zn?
And how about using Urushibara cobalt? Anybody ever tried this catalyst? Cobalt exhibits lower catalytic activity so in this case there would be
possibility to get better selectivity because imines are easier to reduce than aldehydes and ketones.
|
|
karlos³
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1520
Registered: 10-1-2011
Location: yes!
Member Is Offline
Mood: oxazolidinic 8)
|
|
Look, heres my reduction of an oximinoketone to aminoalcohol EXACTLY like in the patent(have you read it, it is a good read?).
First, made solution 1, and dissolved
-2g/8mmol Nickel acetate
in
-10ml Water
Solution 2 was made from ~5ml EtOH and
-3,8g Isonitrosopropiophenone(23,3mmol), added
-55ml NH3 20%(308mmol) and then
-1g KOH in 2ml H2O
to solution 1 then
-6g Zn(92mmol)
were added, and around 15 minutes later, solution 2 was added in portions but over around 25min instead of the 2-3 hours in the patent(but compared,
they used 3l solution with 200g nitroketone in there).
It has not warmed up that much, so a bit heat in the waterbath was added to reach 60°C for 20mins.
Then left stirring for a 6h more.
The precipitate was vacuum filtered and and is washed with 3x15ml dH2O
It was then based with some sodium carbonate and the base extracted using 3x50ml toluene, from which after washing and drying, the oxalate salt was
precipitated.
Drying of that afforded 4,2g(17,7mmol, 76%!), some of this was dissolved in H2O, based and re-extracted with DCM and the HCl the salt formed, which
had a mp of 190-192°C(i.e. it indicates this is the dl-norephedrine).
You really should just read the patent man.
[Edited on 27-1-2020 by karlos³]
|
|
goldberg
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 90
Registered: 28-4-2018
Member Is Offline
Mood: No Mood
|
|
@karlos³: unfortunately this patent is in french and i do not speak french. Second recreation of patent is not always an obvious thing.
So i this case nickel ions became complexed by ammonia and thats why nickel does not precipitate as hydroxide?
Does this procedure works for synthesis of secondary and trietriary amines?
Ni2+ does not have to form complex with more complicated amines.
|
|
Tsjerk
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 3026
Registered: 20-4-2005
Location: Netherlands
Member Is Online
Mood: Mood
|
|
Quote: Originally posted by goldberg ![](images/xpblue/lastpost.gif) | @karlos³: unfortunately this patent is in french and i do not speak french. Second recreation of patent is not always an obvious thing.
So i this case nickel ions became complexed by ammonia and thats why nickel does not precipitate as hydroxide?
Does this procedure works for synthesis of secondary and trietriary amines?
Ni2+ does not have to form complex with more complicated amines. |
Nickel can't precipitate as the hydroxide if it is not oxidized...
https://translate.google.com
Edit: zinc is kept in solution by the ammonia though.