Author: Subject: Tungsten metal plus piranha solution?
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 25-8-2019 at 05:06


Panache:

You can stop making comments supporting my postulated electrochemistry (a new thread/pictures/results soon available exploring a related, but I suspect inferior to the ammonia cell, which I proposed above is likely one of the better path).

Anodic corrosion apparently works more efficiently when the relative surface area of the metal anode, here Tungsten, in my proposed ammonia/H2O2 or O2 electrochemical cell scheme is small. To repeat, when the relative electrode surface area ratio is SMALL (hence low surface area metal Tungsten), say, to the solution's surface area contact with air, the anodic corrosion accelerates.

The cell may create an electric current and associated solvated electrons, e-(aq), so with preferentially added NH4Cl or the sulfate via:

NH4+ = H+ + NH3

And, the removal of H+:

e-(aq) + H+ = .H

the latter two reactions occurring in solution could supply added NH3 (and I would further guess that starting with the highest ammonia concentration is likely not optimal and having the right NH4+ concentration is a factor, see https://www.sciencedirect.com/science/article/abs/pii/S03043... which discusses optimal leaching factors).

[Edited on 25-8-2019 by AJKOER]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 30-10-2019 at 07:23


Quick update on this after a couple of months.
I had originally set up an experiment with a 2g fragment of tungsten, plus H2O2 (27%) and NH4OH (30%). Then I forgot about it.
I found that beaker again last week. All liquid had evaporated (must have been 20ml or so) and the tungsten rod, which initially had showed just a little mass loss, had completely disappeared. What was left was a yellow mass at the bottom, which I thought at first to be crystalline. At closer examination they aren't crystals but irregular pieces that appear like dried-out and broken jello. They are translucent, and I assume they are a mix of ammonium paratungstate (which is white) and tungsten trioxide and/or tungstic acid (which are bright yellow).

I haven't worked that up yet. I'm surprised how well it worked to dissolve all of the tungsten.

But in the meantime I set another experiment up, larger scale. In 2 flasks I added 20g of tungsten pieces each, followed by 25ml of 27% H2O2 each, and in one of them also 5ml of 30% NH4OH. Initially the flask with ammonia heated up a lot and started boiling, almost boiling over despite being a fairly large (500ml) flask. The color of the liquid changed to pale yellow. The other flask with only H2O2 only showed very little gas bubble formation at the surface of the tungsten, which ceased by the next day.

Next morning the yellow color in the ammonia flask had faded, both flasks had a very slightly yellow solution.

Left with ammonia, right without.

I added 6ml H2O2 to each, and in the flask with ammonia the yellow color suddenly intensified. No color change in the one without ammonia. Also no gas bubble formation in either.


I kept the same pattern daily; each day adding 6ml H2O2 in each flask, and every other day 1ml of NH4OH to the left flask only (I keep that one covered with parafilm to minimize ammonia loss). The same phenomenon kept occurring, loss of color by the next day and color intensifies in the left flask as soon as more H2O2 is added. The color in the right flask doesn't change upon addition, just slowly becomes more yellow from day to day.

Flasks on the 3rd day before and after additions:




I noticed that in the left flask (with ammonia) a very fine, dust-like, off-white precipitate has started to form. The precipitate does not change color when I add more H2O2.

No pics on day 4. Here are pics from today, which is day 5. The color changes have become a lot more intense, and there is a lot more of the precipitate.
Before:




And after H2O2:




So far each flask has received 55ml of 27% H2O2, and the left flask only got a total of 8ml 30% NH4OH.

I will keep adding reagents in the same pattern for another 5 days then will just observe.





[Edited on 30-10-2019 by stamasd]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 31-10-2019 at 04:34


Pics from this morning.

Before:



Added ammonia (1ml) in the left flask only; no color change.



Added H2O2 (6ml) to both; yellow color reappears in the left flask.

View user's profile View All Posts By User
Herr Haber
International Hazard
*****




Posts: 1236
Registered: 29-1-2016
Member Is Offline

Mood: No Mood

[*] posted on 31-10-2019 at 04:47


Hello stamasd !

I have tungsten in almost every possible form except plate / foil.
I have all the reagents you used in your experiments and more.
Most important: I have a little bit of space

So if there's an experiment you are not doing for lack of space, time or reagents let me know.




The spirit of adventure was upon me. Having nitric acid and copper, I had only to learn what the words 'act upon' meant. - Ira Remsen
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 31-10-2019 at 05:51


I have space and reagents, time however is another matter... I happen to have some time right now though. Thanks for the offer!
The next thing I plan to try is to see if I can speed up the tungsten dissolution using electrochemistry. But that won't be until this experiment is over.
View user's profile View All Posts By User
wg48temp9
National Hazard
****




Posts: 787
Registered: 30-12-2018
Location: not so United Kingdom
Member Is Offline


[*] posted on 31-10-2019 at 07:39


Molybdenum can also be dissolved with H2O2. If the Mo is in excess when the H2O2 has all reacted to form Mo acid the Mo metal then reduces the acid to a Mo blue.

See the image below from a thread titled "blue tungstic or Molybdic acid ?"

files.php.jpg - 12kB




I am wg48 but not on my usual pc hence the temp handle.
Thank goodness for Fleming and the fungi.
Old codger' lives matters, wear a mask and help save them.
Be aware of demagoguery, keep your frontal lobes fully engaged.
I don't know who invented mRNA vaccines but they should get a fancy medal and I hope they made a shed load of money from it.
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 1-11-2019 at 16:53


Hmm. No pics today, but...
I spent a little time looking at the 2 flasks and I noticed something interesting, which I had not observed until today.
The second flask, the one with only H2O2 and no ammonia, which does not exhibit any color changes when I add more reagent to it, may be in fact more interesting than the other one.
What I noticed is that in that second flask there is now definitely less metallic tungsten remaining compared to the other one. They both started with the same amount (20g) of fragments from 2mm tungsten rods.
Well, the rods in flask 2 are now significantly thinner than the ones in flask 1. I'd say they're no more than 1mm in diameter. :)
If I'm right, they should completely dissolve in the next 3-4 days.
We'll see.

[Edited on 2-11-2019 by stamasd]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 2-11-2019 at 11:29


Okay update with some very interesting information and some calculations.

I pulled out all of the remaining metallic tungsten in both flasks and dried it separately. I was right, the pieces in the H2O2 alone are much thinner and lighter. Here are some photos for comparison.

Left, H2O2+NH4OH; right, H2O2 alone.


Same but closer look.


I then weighed the metal separately. The initial weight was 20.0g for both samples.

The metal from H2O2+NH4OH:


The metal from H2O2 alone:


So in 8 days, the H2O2+NH4OH dissolved 1.3g, whereas the H2O2 alone dissolved 13.8g. Or 0.1625g/day and 1.725g/day respectively.

The NH4OH is actually detrimental to the rate of reaction, slowing it down more than 10x.
View user's profile View All Posts By User
fusso
International Hazard
*****




Posts: 1922
Registered: 23-6-2017
Location: 4 ∥ universes ahead of you
Member Is Offline


[*] posted on 2-11-2019 at 12:28


I wonder if you only add a little NH3 after considerable amount of W is oxidsed, to dissolve most of the oxides, will the dissolved tungstates affect the rate?
Also how does aq NH3 slow down the rxn? Is it due to the extra water or NH3/tungstates decomposing the H2O2?




View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 2-11-2019 at 12:37


I don't have an explanation, these are just my observations. If I were to guess, I'd venture to say that the rate of decomposition of the H2O2 is probably higher in the presence of ammonia. Also apparently no ammonia is needed to dissolve the oxidation product as the solution in the flask with only H2O2 is perfectly clear, if only slightly yellowish but with no visible precipitates.

[Edited on 2-11-2019 by stamasd]
View user's profile View All Posts By User
wg48temp9
National Hazard
****




Posts: 787
Registered: 30-12-2018
Location: not so United Kingdom
Member Is Offline


[*] posted on 2-11-2019 at 15:50


H2O2 is oxidising in acid but in alkali it can be reducing. So I guess if you put too much ammonia in the H2O2 will not oxidize the W or the oxidation rate will be reduced.



I am wg48 but not on my usual pc hence the temp handle.
Thank goodness for Fleming and the fungi.
Old codger' lives matters, wear a mask and help save them.
Be aware of demagoguery, keep your frontal lobes fully engaged.
I don't know who invented mRNA vaccines but they should get a fancy medal and I hope they made a shed load of money from it.
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3035
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 3-11-2019 at 04:01


How would hydrogen peroxide be reducing? I can only imagine it being oxidized by something like fluorine or chlorine trifluoride.
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 3-11-2019 at 06:16


2 KMnO4 + 3 H2O2 --> 2 MnO2 + 2 KOH + 2 H2O + 3 O2

Mn(VII) is reduced to Mn (IV) by the oxygen in H2O2, which itself is oxidized to O2.

[Edited on 3-11-2019 by stamasd]
View user's profile View All Posts By User
Mesa
Hazard to Others
***




Posts: 264
Registered: 2-7-2013
Member Is Offline

Mood: No Mood

[*] posted on 8-11-2019 at 05:27


Fastest/easiest way to dissolve W... Make a thermite-like rxn with NaOH or KOH and dissolve the resulting ash in H2O2.
Alternatively, if you can get it as a powder, ignite a pile of it in open air with a lighter flame, and spread the pile around while it slowly turns red hot, then cools to a fluffy-er yellow WO3 powder.

Reaction is self sustaining with any fine grit W or carbide powder.
Note: if carbide is used, you might have to separate any trace cobalt or molybdenum compounds. Not quite sure though. I only saw it happen in workplace fuckups at my old job. Never tried igniting WC intentionally myself
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 8-11-2019 at 15:34


I don't have a cheap source of powdered W or WC. My W is in the form of broken 2mm rods. I'd also prefer if the resulting WO3 is not contaminated with other chemicals if possible.

Also, as someone else says, I like to explore the science of it. I haven't seen the color change yellow/colorless/yellow mentioned anywhere else, nor the kinetics of W dissolution in acidic vs alkaline conditions.
View user's profile View All Posts By User
Mesa
Hazard to Others
***




Posts: 264
Registered: 2-7-2013
Member Is Offline

Mood: No Mood

[*] posted on 8-11-2019 at 15:53


You could probably just dissolve the ash in conc. NaOH to get sodium tungstate and whatever Na products formed, then treat with HCl to precipitate WO3, all Na products remain soluable.

Without trying it myself I'm not so sure it would dissolve. I'm pretty confident that the HCl step would effectively isolate WO3 product though. No other products could form from the thermite form from HCl except NaCl and H2WO4(decomposes to WO3 in H2O) right?

[Edited on 8-11-2019 by Mesa]

EDIT: There's a pretty easy method to purify any soluable tungsten compound.

Make the ammonium tungstate from HCl + tungstate, separate crystals and redissolve in ammonia solution, evaporate, then fire in open crucible til ammonia stops evolving.
This should work to purify the WO3 you've produced also. In case there is any impurities from electrodes.

I'll post patents when I get on home computer.

[Edited on 9-11-2019 by Mesa]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 9-11-2019 at 03:00


But then I wouldn't be investigating which compound I get from dissolving tungsten in plain H2O2, as I plan on doing soon. You'd think it would be either WO3 and/or H2WO4, but these are bright yellow and completely insoluble. Whereas what I got is a perfectly clear solution that is almost colorless, only a very pale yellow. And that despite having almost 20g dissolved tungsten per 100ml. Whatever is the tungsten species I have (and I'm open to suggestions as to what it is) it's highly soluble.
View user's profile View All Posts By User
Mesa
Hazard to Others
***




Posts: 264
Registered: 2-7-2013
Member Is Offline

Mood: No Mood

[*] posted on 14-11-2019 at 04:40


The solution will precipitate out WO3 over time. I'm not sure what the dissolved species is, except that its unstable in solution and eventually degrades to insoluble WO3 if left alone.
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 14-11-2019 at 19:51


Actually I'm not so sure about that. I haven't touched the flasks for 4 days and their appearance is unchanged as far as the liquid is concerned, only the little bit of tungsten left still undissolved is getting progressively smaller. The liquid is still perfectly clear and very slightly yellow. In a few places it has splashed on the walls and the drops evaporated leaving behind a white deposit with no yellow tinge at all.

[Edited on 15-11-2019 by stamasd]
View user's profile View All Posts By User
Mesa
Hazard to Others
***




Posts: 264
Registered: 2-7-2013
Member Is Offline

Mood: No Mood

[*] posted on 14-11-2019 at 20:59


Try adding a few drops of HCl.
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 15-11-2019 at 05:31


I'll do that in a small sample when all the tungsten is dissolved. The rate of dissolution has slowed down considerably but there is less than half a gram left so it shouldn't take more than a few days.
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 20-11-2019 at 16:35


Only 2 small pieces of tungsten remain, about 0.5mm thick and 3-4mm long each.

View user's profile View All Posts By User
Mesa
Hazard to Others
***




Posts: 264
Registered: 2-7-2013
Member Is Offline

Mood: No Mood

[*] posted on 21-11-2019 at 23:29


Likely some kind of peroxo tungstic acid such as described in this link

Evaporating the water at no more than 100*c will isolate the pertungstic acid. Heating above 100*c will decompose it to WO3.

Could explain the precipitate on the side of the flasks?


EDIT: This link seems to be more relevant
https://www.researchgate.net/post/How_can_I_get_a_clear_solu...

[Edited on 22-11-2019 by Mesa]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 22-11-2019 at 07:56


I can't use the first link "you have reached a page that's unavailable for viewing"
As for the second link, it describes the second part of the experiment (the left flask in some of the pictures above) with H2O2+ammonia, which showed a dissolution rate 10x slower than plain H2O2.

But yes, it's probable that what I'm getting is an adduct between WO3 and H2O2 aka peroxopolytungstic acid.

[Edited on 22-11-2019 by stamasd]
View user's profile View All Posts By User
stamasd
Hazard to Others
***




Posts: 137
Registered: 24-5-2018
Location: in the crosshairs
Member Is Offline

Mood: moody

[*] posted on 26-11-2019 at 13:52




The tungsten dissolution is complete. I have set the solution to evaporate.
View user's profile View All Posts By User