Destructive distillation of polypropylene


Some years ago I collected together a large quantity of waste polypropylene (PP) plastic in the form of yoghurt pots for the purpose of pyrolysis. I had discovered a book section[1] which detailed the products of thermal decomposition of polymers. This stated that the products of thermal decomposition of polypropylene were "...pentane (24 percent), 2 methyl-1-pentene (15 percent), and 2–4 dimethyl-1-hep-tene (19 percent)." It was on this basis that I planned to pyrolyse a quantity of polypropylene followed by fractionation for these high-value products. It seems, however, from my own experiments that the result under my conditions more closely resembled crude oil.

Earlier this month I finally got around to shredding about a third of them into small enough pieces to fit through the neck of a bottle.
I bought a cheap 500 mL stainless-steel water bottle and filled it as full as I could with chopped PP, stoppered it with a sparkling wine cork and set up for distillation with a gas burner. Once the charge of plastic had been exhausted, the cooled steel bottle appeared empty without any char, fortunately. I then refilled it, and repeated several times until I had destructively distilled all 660 g of chopped plastic. I found that cork was a poor choice of stopper for the high temperatures involved, and I turned to a sacrificial rubber bung instead. After about half a dozen runs (the whole lot), the rubber stopper was in no fit state for anything, and was thrown away.

My yield of pyrolysis oil was 650 mL, with a density of 0.701 g/mL at about 22°C (est.).

This oil was then simply distilled, and crudely fractionated into six fractions:
rt 2 L (est.)
35-85°C 50 mL
85-135°C 50 mL
135-155°C 70 mL
150-250°C (est.) 400 mL
250-300°C (est.) 40 mL
300+°C (est.) 40 g

My thermometer does not go above 150°C, hence estimated temperatures based on vegetable oil viscosity of the penultimate fraction. The fractions were dried over calcium chloride, with the higher boiling ones taking much longer to dry than the lightest. The final result was five crystal-clear liquids, darkening to olive-oil coloured for the 250-300°C fraction. The final "fraction" was the residue left in the flask, and is the colour of black treacle with a consistency of hard vaseline.

The first fraction to boil out of solution was not condensed by an ice-water-cooled double-surface Leibig condenser, I concluded that this was petroleum gas, comprising (presumably) ethylene, propane, propylene, butane, and butenes. I was not expecting this, so I cannot confirm or deny if alkenes were present in this gas.

Based on these results, I would propose that the pyrolysis oil of polypropylene serves a remarkably cheap and safe alternative to crude oil for educational purposes, and contains a full range of crude oil fractions, without carcinogenic aromatics like benzene. This later assertion is based on the C:H ratio in the feedstock plastic compared to the C:H ratio of aromatic compounds. A considerable amount of hydrogen would have to be released for this class of compound to be formed, which is unlikely under the conditions.

[1] C. L. Beyler and M. M. Hirschler, Chapter 7, SPE Handbook of Fire Protection Engineering, 2001, pp. 110–131.

Attachment: Beyler, Hirschler - 2001 - Thermal Decomposition of Polymers(2).pdf (165kB)
This file has been downloaded 494 times

My set-up for pyrolysis:
2019-08-25 - Copy.png - 763kB




Just my two pennyworth
My YouTube channel: www.youtube.com/channel/UC4t9tVlAk7ww1wgCVW4yUjg
Elements collected so far: 65; to collect: Ln, Rb, Sr, Ba, F, Kr, radioactives
View user's profile Visit user's homepage View All Posts By User
hissingnoise
International Hazard
*****




Posts: 3940
Registered: 26-12-2002
Member Is Offline

Mood: Pulverulescent!

[*] posted on 25-8-2019 at 12:21


I thought yogurt pots were made of polystyrene (vinylbenzene).

View user's profile View All Posts By User
12thealchemist
Hazard to Others
***




Posts: 181
Registered: 1-1-2014
Location: The Isle of Albion
Member Is Offline

Mood: Rare and Earthy

[*] posted on 26-8-2019 at 01:07


In my case, they're polypropylene:

IMG_20190826_095835-min.jpg - 822kB

I've done destructive distillation of polystyrene before, and that produces a completely different product with a very different and distinctive smell. The pyrolysis oil described here has a petroleum odour, similar to fuel (fuel meaning petrol, diesel, kerosene, etc.)

[Edited on 26-8-2019 by 12thealchemist]




Just my two pennyworth
My YouTube channel: www.youtube.com/channel/UC4t9tVlAk7ww1wgCVW4yUjg
Elements collected so far: 65; to collect: Ln, Rb, Sr, Ba, F, Kr, radioactives
View user's profile Visit user's homepage View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 26-8-2019 at 01:29


Excellent work.if the resulting oil you obtained is similar to that list of products once the pentane is distilled off and the resulting alkenes reduced to alkanes you should have a mixture quite similar to petrol which when done on a large scale would prove quite profitable.a video I seen on YouTube of a bench top model pyrolysis unit that spits out a petroleum substitute was using a polypropylene/polyethylene 90% 10%polycarbonate mix.
View user's profile View All Posts By User
12thealchemist
Hazard to Others
***




Posts: 181
Registered: 1-1-2014
Location: The Isle of Albion
Member Is Offline

Mood: Rare and Earthy

[*] posted on 26-8-2019 at 01:58


The resulting oil appears to be completely different to the list of products given. Almost no pentane was collected, and 60% of the oil boiled at a temperature above that of the highest-boiling component of the list. As I described, the composition of the oil I obtained was closer to that of crude oil than that of petrol.



Just my two pennyworth
My YouTube channel: www.youtube.com/channel/UC4t9tVlAk7ww1wgCVW4yUjg
Elements collected so far: 65; to collect: Ln, Rb, Sr, Ba, F, Kr, radioactives
View user's profile Visit user's homepage View All Posts By User
Ubya
International Hazard
*****




Posts: 1247
Registered: 23-11-2017
Location: Rome-Italy
Member Is Offline

Mood: I'm a maddo scientisto!!!

[*] posted on 26-8-2019 at 02:36


pyrolisis produces a big range of molecules, a long chain like PP can break forming different chain length molecules, i would be surprised if the products were only 3 and with pretty short chains, maybe with higher temperature or a catalyst you can get smaller chains, but in general you'll never be able to get just one or a few molecules from the pyrolisis of a big polymer.




---------------------------------------------------------------------
feel free to correct my grammar, or any mistakes i make
---------------------------------------------------------------------
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5109
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 26-8-2019 at 07:15


Quote: Originally posted by 12thealchemist  

contains a full range of crude oil fractions, without carcinogenic aromatics like benzene. This later assertion is based on the C:H ratio in the feedstock plastic compared to the C:H ratio of aromatic compounds. A considerable amount of hydrogen would have to be released for this class of compound to be formed, which is unlikely under the conditions.




Not really.
Two observations- you produced coke/ char.
If you can get carbon, you can get aromatics.

Also, you can "lose" hydrogen by breaking long carbon chains.#
I'm not saying this sort of reaction
C14 H30 --> C6H6 + 4 C2H6
is common, just that it's possible.
View user's profile View All Posts By User
draculic acid69
International Hazard
*****




Posts: 1371
Registered: 2-8-2018
Member Is Offline


[*] posted on 26-8-2019 at 08:22


He said there was no char leftover in the vessel after pyrolysis.
View user's profile View All Posts By User