Preparation of STABLE colloidal gold


For my element collection I also want to add small samples of colloidal gold. I know how to make this from HAuCl4 and Na-citrate, but the solutions tend to be unstable on storage. Over time, the particles tend to aggregate into larger ones and settle at the bottom.

Maybe someone else over here has experience in making stable colloidal gold "solutions" which can be ampouled and stored indefinitely?

I have a 4% solution of HAuCl4 as starting material. I want the red variation and the blue/purple variation, the latter having IIRC a larger particle size.




The art of wondering makes life worth living...
Want to wonder? Look at https://woelen.homescience.net
View user's profile Visit user's homepage View All Posts By User
j_sum1
Administrator
********




Posts: 6279
Registered: 4-10-2014
Location: Unmoved
Member Is Offline

Mood: Organised

[*] posted on 24-3-2016 at 00:38


Snap.
I have exactly the same idea for m collection.
I am also interested in something that lasts long term. I have heard of a very large number of agents used for colloidal gold but don't know much about of any of them.




View user's profile View All Posts By User
CuReUS
National Hazard
****




Posts: 928
Registered: 9-9-2014
Member Is Offline

Mood: No Mood

[*] posted on 24-3-2016 at 04:16


this might be useful
https://en.wikipedia.org/wiki/Gold_number
View user's profile View All Posts By User
unionised
International Hazard
*****




Posts: 5116
Registered: 1-11-2003
Location: UK
Member Is Offline

Mood: No Mood

[*] posted on 24-3-2016 at 05:54


The colloidal gold that stained my kitchen counter-top was so stable that I ended up painting over it to cover the purple stain.
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3663
Registered: 8-2-2015
Location: 3rd rock from the sun
Member Is Offline


[*] posted on 24-3-2016 at 06:46


I do not know anything about colloidal gold but I have made and stored colloidal silver
by simply passing a current through two silver electrodes in distilled water
The initial megohms of resistance drops VERY quickly as ions enter the water
More coulombs gives more suspended (and I believe ionic) silver in the water
Continued current starts to grow the size of the colloidal particles after about 20 ppm.

Caution: from memory, please verify.
View user's profile View All Posts By User
Oscilllator
National Hazard
****




Posts: 659
Registered: 8-10-2012
Location: The aqueous layer
Member Is Offline

Mood: No Mood

[*] posted on 24-3-2016 at 14:34


I'm sure you have already thought of this, but why not try using an emulsifier?
A quick google search seems to suggest there are lots of them readily available because they are used in food products, so it's worth a shot surely.
View user's profile View All Posts By User
Sniffity
Hazard to Self
**




Posts: 70
Registered: 27-12-2014
Member Is Offline

Mood: No Mood

[*] posted on 25-3-2016 at 19:10


Hey,

Might not be exactly what you're looking for; but gold nanoparticles can be prepared using a certain polymer, chitosan, as a reducing and capping agent. I've seen this experiment succesfully replicated at our polymers lab in my university. The red colour you wish to obtain was clearly visible. I'm not sure about long term storage, but in chitosan does seem to be good at stabilization of a large number of compounds.

Here's the scientific paper we used as reference for this experiment:
http://www.sciencedirect.com/science/article/pii/S0167577X14...

I happen to have this paper in Pdf format, but I have no idea how to upload here. If anyone lets me know of a way to share it, I gladly will.

Hope this helps!
View user's profile View All Posts By User
Tsjerk
International Hazard
*****




Posts: 3028
Registered: 20-4-2005
Location: Netherlands
Member Is Offline

Mood: Mood

[*] posted on 26-3-2016 at 01:14


Maybe coupling with bovine serum albumin (BSA) would work? This protein is really stable and is regularly used as coating for hydrophobic (e.g. plastic) surfaces in order to prevent adhesion of hydrophobic dyes. I could imaging BSA will prevent particles to aggregate.

http://openwetware.org/images/c/c9/110417_SDP_TannicAcidAuNP...

In this method dialysis of the sample is described, but that would be unnecessary if it is just to prevent aggregation during storage I guess.

If you think this could be a solution I could sent you a milliliter of solution, as we get these tubes included with about every order we make.

[Edited on 26-3-2016 by Tsjerk]
View user's profile View All Posts By User
fluorescence
Hazard to Others
***




Posts: 285
Registered: 11-11-2013
Member Is Offline

Mood: So cold outside

[*] posted on 26-3-2016 at 04:28


I didnt even know it reacted. There was a good paper on the preparation of diferent sizes of collodial Gold since elemental gold nano particles can be used for a visible light with TCPO, that is actually quite cool in the mechanism. So they tried different ways how to reduce the gold in different sizes. Maybe changing to bigger particle size could improve the stability ?

http://pubs.acs.org/doi/abs/10.1021/ac050882q
View user's profile View All Posts By User
Chalo
Harmless
*




Posts: 15
Registered: 31-7-2017
Member Is Offline

Mood: Hopeful

[*] posted on 21-8-2022 at 13:16


The most stable gold nps involve self-assembled-monolayers that coat the particle and keep them from sticking together as aggregates; even better if the particles are charged and repel each other; and still better if they are in a nonpolar solvent like hexane that increases the repulsion. Particles like that were a bear to make, taking days and exotic detergents and $$$, or you could buy them from sigma for a kilobuck per 5 mls. BUT!!! recently someone published a ten minute inexpensive protocol. These could be ampouled indefinitely and are beautiful.

I have the pdf but dont know how to upload it.

See video:https://www.youtube.com/watch?v=nqkwM9o1s-w

see paper: Charged Gold Nanoparticles in Non-Polar Solvents: 10-min Synthesis and 2D Self-Assembly
Matthew N. Martin, James I. Basham,† Paul Chando, and Sang-Kee Eah*
View user's profile View All Posts By User
clearly_not_atara
International Hazard
*****




Posts: 2761
Registered: 3-11-2013
Member Is Offline

Mood: Big

[*] posted on 24-8-2022 at 16:56


Stained glass ;)



Quote: Originally posted by bnull  
you can always buy new equipment but can't buy new fingers.
View user's profile View All Posts By User
Chalo
Harmless
*




Posts: 15
Registered: 31-7-2017
Member Is Offline

Mood: Hopeful

[*] posted on 26-8-2022 at 17:24


Figured out how to attach the paper here.
could not get this to work, NaBH4 reacts instantly but also aggregated instantly into tiny dark blue spheres.
Hope someone else tries this. If you need dodecanethiol, I have 100 mls, so given only a microliter needed per reaction I can spare enough for a few thousand reactions.

The applications for stable AuNPs, especially as redox catalysts, are endless check literature.

Attachment: goldnano martin2010.pdf (2.1MB)
This file has been downloaded 273 times

Untitled-1.jpg - 170kB
View user's profile View All Posts By User
Sulaiman
International Hazard
*****




Posts: 3663
Registered: 8-2-2015
Location: 3rd rock from the sun
Member Is Offline


[*] posted on 27-8-2022 at 01:27


I noticed that gold precipitated from chloroauric acid gives smaller particles at lower acid concentrations.
Try working with more (100x?) dilute solutions?




CAUTION : Hobby Chemist, not Professional or even Amateur
View user's profile View All Posts By User
pneumatician
Hazard to Others
***




Posts: 409
Registered: 27-5-2013
Location: Magonia
Member Is Offline

Mood: ■■■■■■■■■■ INRI ■■■■■■■■■■ ** Igne Natura Renovatur Integra **

[*] posted on 8-11-2022 at 18:06


maybe a "tincture"/extraction of Gold with ether???

this guy use Rosemary oil = colloidal Au

https://vimeo.com/142743073

or...

https://www.youtube.com/watch?v=MDF2TXZIuj0

this precipitate/go rancid/ferment...??? I don't known till I make a test :-)
View user's profile View All Posts By User
Junk_Enginerd
Hazard to Others
***




Posts: 250
Registered: 26-5-2019
Location: Sweden
Member Is Offline


[*] posted on 17-11-2022 at 07:49


This makes me think of NileRed's video about preparing ferrofluid. That's also a case where the particles really want to aggregate, but are stopped from doing so by coating the nanoparticles with soap molecules. It should be just as applicable to gold particles.
View user's profile View All Posts By User
clearly_not_atara
International Hazard
*****




Posts: 2761
Registered: 3-11-2013
Member Is Offline

Mood: Big

[*] posted on 17-11-2022 at 21:21


Most emulsions need surfactants to stabilize them.



Quote: Originally posted by bnull  
you can always buy new equipment but can't buy new fingers.
View user's profile View All Posts By User
Lithium
Hazard to Others
***




Posts: 103
Registered: 25-2-2012
Location: Australia
Member Is Offline

Mood: Thinking!

[*] posted on 19-11-2022 at 19:37


Colloidal systems are inherently unstable. Particles dispersed in solution have a tendency to aggregate: think of paint, of milk, of muddy river water. Colloids aggregate over a wide range of timescales: seconds, hours, weeks, years. But they all do. A variety of tweakable features have a role to play: particle size, the composition of the continuous medium, the composition of the particle and the particle's surface. I will briefly discuss them in turn.

Aggregation is driven by entropy, or thermodynamics, or both. When a bulk material is dispersed as finely divided particles in a continuous medium, the interfacial area between those two mediums is made much much larger. A grain of gold divided into nanosized particles and dispersed into water has a significantly larger area where the gold atoms are in contact with water molecules. Because 'like favours like', the gold atoms prefer contact with other gold atoms and the water molecules prefer contact with other water molecules. As a consequence, it is thermodynamically favourable for the system to reduce the area of contact between gold atoms and water molecules.
Increasing this area is rolling the ball up the hill. The ball tends toward the bottom.

Broadly speaking, nanoscale particles tend to aggregate less frequently. For example, clinically-used liposomal preparations are on the order of 200 nm in diameter or less. Particles of this size take longer to aggregate; greater biocompatibility and a longer circulation half-life is evidence of this. The substantially reduced tendency toward aggregation is a unique feature of nanoscale materials which is partly responsible for the recent explosion in their study. Size matters.

The composition of the continuous medium matters. Specifically, the species that are also present in the continuous medium. Ionic substances substantially influence aggregation rates. In the case of NaCl, higher concentrations promote aggregation. This effect can be dramatic. Charged species disrupt the electric double layer that naturally forms around a colloidal particle, causing a charge-screening effect that reduces the repulsive forces between particles. This effect can also be seen with proteins and peptides that adhere to the particle's surface. Note that some ionic species such as Li+ and F- have outlier-type effects on this layer.

The composition of the particle matters, but mainly because it decides what you can stick to the surface and how. Steric stabilisation is possibly one of the most widely used or effective techniques to improve the stability and shelf-life of colloidal systems. Their mechanism is very simple: two particles can't aggregate if they don't touch. There are two broad types: surfactants bound to the particle itself, and surfactants in the continuous medium that naturally stick to the surface of the particle. The first is more reliable or robust; the second can be simpler or more practicable to use. They are both very effective.

Aside:
The tried-and-true method for characterising particle size is dynamic-light scattering (DLS). It's rapid, simple, and cheap. I am certain that an amateur could construct an instrument capable of carrying out this technique, if one has not already done so. This is a call to the amateur experimentalist out there with a little more raw material and engineering savviness than most, but who still has some time to tinker. A simple and cheap DLS instrument reproducible by the amateur opens one of three doors to the field of nanoscience. The other two include communicating safe practices for experimentation and handling waste that are unique to nanomaterials, and a technique to gather information on the crystal structure of the material. I'm sure both will take time, the second a lot more than the first.

I am a little rusty on the foundational theory, but there is a lot out there to read on colloid and interface science. Take care.




Li
View user's profile View All Posts By User
pneumatician
Hazard to Others
***




Posts: 409
Registered: 27-5-2013
Location: Magonia
Member Is Offline

Mood: ■■■■■■■■■■ INRI ■■■■■■■■■■ ** Igne Natura Renovatur Integra **

[*] posted on 20-11-2022 at 08:41


Well, the easy method is to tint some water with from yellow to deep purple and say to anybody: hey look, this is colloidal Gold! :-D

or go a bit more deep inside the "secrets" of colloidal metals...

http://www.silvermedicine.org/colloidal-silver-medical.html

https://www.elixa.com/colloidal-silver-a-closer-look/

https://healthwyze.org/reports/633-making-and-using-genuine-...

snake silver oil ha ha ha

https://www.quantumbalancing.com/news/cs_lunar.htm

or go to real Gold "spiritual" better than any colloidal shit, but this is for "quantum" minds only...

[Mode end: pedantic]
--> error no pedantic Mode on
[Mode end: genius]
Ok_
View user's profile View All Posts By User
Lionel Spanner
Hazard to Others
***




Posts: 166
Registered: 14-12-2021
Location: near Barnsley, UK
Member Is Offline


[*] posted on 21-11-2022 at 14:00


In my experience experience, 0.1% low-acyl gellan gum gelled with calcium ions does an excellent job of suspending solids in water and minimising aggregation, while adding little if any viscosity. Never tried using it with colloidal gold or silver though.



Industrial chemist rediscovering the practical pleasures of pure chemistry.
Sometimes I make videos - https://www.youtube.com/@yorkshirechemist
View user's profile View All Posts By User

  Go To Top