[*] posted on 22-9-2015 at 22:24


Very nice work kadriver! I'm so excited to see this after 48h (though a good deal should be off in 24h). Thank you for scaling up!

Yes from the little I could see, the GRF looks like a very large forum, especially considering it's all about one topic. I think info just slips through sometimes. I did notice that those threads lacked some important details. I don't think it was well understood at that point and possible people couldn't reproduce it with the given details and so it lost momentum? Not sure why it went dead so quickly and more investigations not performed. The info on the oxidant was particularly hazy, I think the key here is that bubbling is very important. While the peroxide might work initially, it breaks down quite quickly to water and oxygen in the presence of transition metals which act as catalysts, so it's activity would quickly diminish.

Furthermore, these kinds of important discoveries ought to be highlighted so as to disseminate the information. This additional thread and also your youtube videos should go a long way to publicizing this better.

[Edited on 23-9-2015 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 23-9-2015 at 08:52


Fact that it's been done before, but nobody knew about it tells us something important : publicise your work or it gets forgotten !

Sad to think that vast quantities of PCBs have been dunked in concentrated nitric acid when they could have been doing this instead.

Can't wait to see the video !




View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 28-9-2015 at 02:00


I wonder what happened to kadriver's experiment. It's been many moons now :(



Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 4-10-2015 at 21:13


Hello,

Sorry it took so long. The experiment was progressing nicely, then I got swamped with work.

I left the bubbler in for about 6 days. On day five I noticed a light blue precipitate starting to form in the beaker.

About 98 percent of the foils came off the fingers. I had set the experiment aside to get some important work done.

Then disaster - I dropped a heavy glass lid from another process onto the experiment and broke the 5 liter beaker. It's just set there like that for about a week.

That's usually what happens when I reach a point where I don't know what to do.

Here is a picture.

kadriver

image.jpg - 1.2MB image.jpg - 1.2MB image.jpg - 459kB
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 4-10-2015 at 21:20


Things have calmed down.

There is about 50$ worth of gold foils that I need to get out but I'm not sure how to proceed.

Tomorrow I'll decant the liquid, pick out the shards of glass (the glass saucer I had sitting on top also broke and fell down into the experiment) then transfer to a new container so I can carry on the experiment.

I have no idea what the blue precipitate is. I'll get some samples and start running some tests to see if I can find a solvent that will dissolve the light blue ppt but leave the gold foils.

I have never encountered this type of material, any thoughts on what it might be and how I can dissolve it?

Thanks, kadriver
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 4-10-2015 at 21:37


Sorry to hear about your disaster.

Sounds like the precipitate may contain copper salts. You ought to be able to wash these through a strainer/sieve and retain your gold fingers. After that I suggest filtering the solutions so you can keep the filtrate for the next batch and recover the precipitate.

The precipitate should dissolve in conc. HCl if it doesn't dissolve well in water alone. You might want to try dissolving a small amount in saturated sodium chloride as well to see if that works, it's more benign than conc. HCl and cheaper! If it contains copper(I) in the mix, then that won't be very soluble in water alone.

[Edited on 5-10-2015 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
violet sin
International Hazard
*****




Posts: 1482
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline

Mood: Good

[*] posted on 4-10-2015 at 21:41


might ammonia re-dissolve the copper compound to filter out gold fingers? that is if it is a copper salt we are seeing as the blue ppt.
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 4-10-2015 at 22:04


Quote: Originally posted by violet sin  
might ammonia re-dissolve the copper compound to filter out gold fingers? that is if it is a copper salt we are seeing as the blue ppt.


Oooh, that's going to get really pretty, pretty fast :D Nice idea!

[Edited on 5-10-2015 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 4-10-2015 at 23:10


blimey that must be strong stuff! looks a bit like this


nitrate1.JPG - 138kB
Mine is copper disolved in nitric and sulphuric acid (both conc), so I would say thats copper for sure. Then again I am often wrong :P
mine been there so long the dark blue on the bottom is crystals! what struck me is how similar the white powder was and how it sticks to the sides of the glass

[Edited on 5-10-2015 by Little_Ghost_again]

How much did it evaporate? I only ask because you said about the plate on top, I am wondering if your white powder is salt? but the blue looks like a fair bit of copper

[Edited on 5-10-2015 by Little_Ghost_again]




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 04:34


Quote: Originally posted by deltaH  
Sorry to hear about your disaster.

Sounds like the precipitate may contain copper salts. You ought to be able to wash these through a strainer/sieve and retain your gold fingers. After that I suggest filtering the solutions so you can keep the filtrate for the next batch and recover the precipitate.

The precipitate should dissolve in conc. HCl if it doesn't dissolve well in water alone. You might want to try dissolving a small amount in saturated sodium chloride as well to see if that works, it's more benign than conc. HCl and cheaper! If it contains copper(I) in the mix, then that won't be very soluble in water alone.

[Edited on 5-10-2015 by deltaH]


I noticed the precipitate in very small volumes starting on day two with the bubbler. On day five it exploded exponentially and started to coat the inside of the beaker.

I have some extra fine copper mesh that might work as a strainer. Also a steal tea strainer that has a fine mesh. Straining out the foils and rinsing the ppt through never occurred to me - thanks for that tip.

As for ammonia, I try to keep it out of my processes. It will dissolve silver chloride and that can be useful. But adding it to waste treatment creates a plume of ammonia that is ruinous to equipment and lungs.

I'll get a sample of the blue precipitate and try a few drops of ammonia to see if it will dissolve the copper salt.

I started filming for this video at the beginning. But I usually try to produce the video as the process is going in real time to keep everything fresh. I can do this because I am very familiar with the process and I know what's going to happen next.

But with this I am in unfamiliar territory. I stopped shooting video when the precipitate showed up. Couple that with the broken beaker and it's not looking good for completing this experiment - on video.

I'll probably get the foils from this batch and start the experiment over, being more familiar with what to expect. THEN do a video showing the complete process.

I'll keep this thread posted on how I proceed from here with photos, but probably not a video this time around.

kadriver
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 04:41


Quote: Originally posted by Little_Ghost_again  
blimey that must be strong stuff! looks a bit like this



Mine is copper disolved in nitric and sulphuric acid (both conc), so I would say thats copper for sure. Then again I am often wrong :P
mine been there so long the dark blue on the bottom is crystals! what struck me is how similar the white powder was and how it sticks to the sides of the glass

[Edited on 5-10-2015 by Little_Ghost_again]

How much did it evaporate? I only ask because you said about the plate on top, I am wondering if your white powder is salt? but the blue looks like a fair bit of copper

[Edited on 5-10-2015 by Little_Ghost_again]


I always try to keep a cover of some sort on the beaker. I did not note the amount of evaporation.

I must say that the concept of using vinegar, salt and peroxide is fantastic, the formation of the blue ppt really throws a wrench into the gears of this process. I didn't expect it.

kadriver
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 5-10-2015 at 05:53


Okay, some detective work is in order then.

I must say, I'm doubting that this precipitate is copper(I) now considering that it took so long to form and then formed exponentially. That doesn't fit. If anything, prolonged bubbling should oxidise all the copper (I) to copper (II), which I think it did and that is the blue solution you see, especially after [presumably] all the copper has been leached.

The precipitate is something else, could it be tin oxide and/or lead salts from solder?

[Edited on 5-10-2015 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 5-10-2015 at 07:02


I asked about evaporation because I wondered if the white stuff was salt or maybe lead something. Then again he used fingers I think, so should be no lead as it should be the copper the glue the gold and the stuff they put on top like a varnish (the name escapes me).
How do I make the acetate? mine hasnt turned up.
I am eager to give this another try




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 5-10-2015 at 08:54


What do your mean by "how do I make the acetate"?



Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 5-10-2015 at 09:08


The fact that PCBs have a lot of copper on them surely suggests the blue is a copper salt ?

Also it's Blue ...




View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 5-10-2015 at 13:10


Quote: Originally posted by deltaH  
What do your mean by "how do I make the acetate"?


Sorry was a mix up ignore that.




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
Little_Ghost_again
National Hazard
****




Posts: 985
Registered: 16-9-2014
Member Is Offline

Mood: Baffled

[*] posted on 5-10-2015 at 13:16


Quote: Originally posted by aga  
The fact that PCBs have a lot of copper on them surely suggests the blue is a copper salt ?

Also it's Blue ...

I think the detective stuff is more to do with the white powder, there is alot of it. Could be copper(I) but I am guessing that would be unlikely. The blue as you say has to be copper, and a fair bit going by the colour, if he added alot of conc H2O2 then maybe the white stuff is copper(I)??
I am pretty sure it wont be lead etc as these were fingers, so unless a fair number had some soldering done to them I cant see lead being in there, that leaves the glues and coatings, depending on the number of layers of the boards used that could be a fair bit. I havnt got a clue what they use as a bonding material.
The only other way out idea is maybe the glass fiber resin came out and created the white precipitate. But judging it against mine (whatever that is) it seems to be the same white powder, I am pretty sure mine is copper of some sort as it only had copper and acids added




Dont ask me, I only know enough to be dangerous
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 21:47


Quote: Originally posted by Little_Ghost_again  
Then again he used fingers I think, so should be no lead as it should be the copper the glue the gold and the stuff they put on top like a varnish (the name escapes me).


I did used trimmed clean fingers. I think the green coating is called "solder mask".

I got some more photos to post as soon as my PC updates the virus scan.

View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 22:20


The strainer worked nicely. probably let some of the tiny pieces of gold foils through. But as you can see most are in the strainer!

I was at a loss on how to proceed. Many thanks to deltaH for suggesting the strainer.

P1260481.JPG - 906kB
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 22:23


After getting the foils in the strainer and rinsing the precipitate off into the small bucket, I collected all the foils in a big bucket of water

P1260483.JPG - 2.1MB
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 22:26


Here is all the foils ready to dissolve. Thanks for helping me with this. If not for the suggestions I received here it would still be sitting there untouched and broken!

P1260486.JPG - 2MB
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 22:33


I filtered out the foils and placed them and the filter paper into a 600ml beaker.

I adding about 100ml HCl then adding about 10ml houshold bleach in my fume hood. The foils dissolved in just a few minutes, the filter paper disintegrated.

I then filtered the filter paper and other solids out so I had a clean solution of gold bearing liquid.

I added a couple of spoons of sodium meta bisulfite and the gold precipitated. see photo.



P1260488.JPG - 1.8MB
View user's profile View All Posts By User
kadriver
Hazard to Others
***




Posts: 196
Registered: 7-11-2012
Location: United States
Member Is Offline

Mood: Thankful

[*] posted on 5-10-2015 at 22:40


It was getting late. I'll let the gold settle overnight then collect the gold powder in a filter paper, melt it and post the yield tomorrow.

AGAIN, many thanks for helping me through this. The precipitate threw me for a loop.

Now that I have some time and am familiar with the process i'll make a video and post it on youtube, then add it to this thread.

kadriver
View user's profile View All Posts By User
aga
Forum Drunkard
*****




Posts: 7030
Registered: 25-3-2014
Member Is Offline


[*] posted on 5-10-2015 at 23:26


Brilliant stuff kadriver - Success !

Just think : your video will show how to replace the conc nitric acid currently used in the process, and eliminate an awful lot of seriously toxic fumes, maybe even save a few lives.




View user's profile View All Posts By User
deltaH
Dangerous source of unreferenced speculation
*****




Posts: 1663
Registered: 30-9-2013
Location: South Africa
Member Is Offline

Mood: Heavily protonated

[*] posted on 6-10-2015 at 05:04


Yes, very nicely done kadriver and thanks so much for scaling up! Death to HCl! :D Death to nitric! :D:D

[Edited on 6-10-2015 by deltaH]




Mind your step or step your mind. Website: www.ideashack.org
View user's profile Visit user's homepage View All Posts By User
 Pages:  1  2    4    6  ..  9

  Go To Top