Arc furnace power supply
Recently I have been messing around with arc furnaces again. The power supply I am using right now consists of three MOTs. I have all of the primary
coils hooked in series from the wall (120v), and all of the secondaries shorted. This way the inductive load is split between the three transformers
so they don't heat up too fast. While this design works, I feel that I need more power. Would removing the secondary coils allow for more power? Would
removing the secondary coils make the transformers heat up faster? Do I need to just ditch the MOT method and use something else? Any help is
appreciated!
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
If you need more power you could remove a transformer (assuming the remaining two can handle it).
The shorted secondaries are only wasting power in resistive losses, and can be removed.
|
|
gregxy
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 421
Registered: 26-5-2006
Member Is Offline
Mood: No Mood
|
|
I used to have a cheap welder that plugged into a 110V outlet. The carbon-arc torch that came with it worked quite well. All it had was a resistor
(made from heavy nichrome wire) in series with the power leads. The total resistance was probably 5-10 ohms so the current output would be around 15A.
This is an inefficient way to do it but works if you don't care about wasting power.
A better way would be to remove the secondaries from the MOT and replace them with 10-50 turns of heavy wire creating a step-down transformer. How
many turns depends on the voltage you want the arc-length and other things. Or buy a cheap welder.
|
|
WChase501
Harmless
Posts: 16
Registered: 23-1-2014
Location: Hot Springs Arkansas
Member Is Offline
Mood: Depressed and Happy
|
|
A welder only has a limited amount of time that it can work. If you buy a cheap one, for example the usable time would be lets say 3 mins out of 10
mins, would that be enough time for you to perform your work?
|
|
WChase501
Harmless
Posts: 16
Registered: 23-1-2014
Location: Hot Springs Arkansas
Member Is Offline
Mood: Depressed and Happy
|
|
Also Neon sign transformers can be rewound just like a microwave oven transformers. NST though can be used in a shorted out environment for
substantial periods of time without overheating just fyi. If you need more information please contact me.
|
|
Dan Vizine
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 628
Registered: 4-4-2014
Location: Tonawanda, New York
Member Is Offline
Mood: High Resistance
|
|
What type of supply is used in industry?
I would have guessed DC may be preferred (with the non-consumable electrode negative)?
High power rectifiers are fairly inexpensive, if this is the case.
|
|
Lambda-Eyde
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 859
Registered: 20-11-2008
Location: Norway
Member Is Offline
Mood: Cleaved
|
|
Overheating can easily be solved by submersing the transformers in an appropriate oil, which, if needed, can be cooled by circulating it through a
Al/Cu radiator.
This just in: 95,5 % of the world population lives outside the USA
You should really listen to ABBAPlease drop by our IRC channel: #sciencemadness @ irc.efnet.org
|
|
violet sin
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1477
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline
Mood: Good
|
|
I cam across this the other day: http://blog.modernmechanix.com/mags/PopularScience/5-1933/ar...
it shows how to make your own current limiting reactance from laminate steel pieces and copper wire. says it is an improvement from using a toaster
(or two) to limit the current. as only about 3 amperes flows with the toaster method, and only maxed out when the carbon tips are touching. the
reactance device upsets the power factor and gets about 10 amperes flowing through the arc, even though only 3.5 amperes are measured as flowing in
the circuit.
the inductor was specially designed for the hobby arc melter, not just a re-purposed device.
( all from the article ^^^)
I have never got around to trying it yet, but it looks promising.
-Violet Sin-
|
|
markx
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline
Mood: Very Jolly
|
|
Depending on what kind of output power and duration (duty cycle) is required for the experiment I would suggest opting for an inverter arc welder. The
cheaper ones do not cost that much nowadays and one can really get some performance out of them if you run on low power.
The MOT method calls for at least 2 of them connected in series to get a decent inductive load for the primary winding and a custom wound secondary,
but the whole assembly becomes bulky, heavy and is still quite ineffective in terms of power conversion.
I did experiment with the MOT's while I tried to find a suitable high amp power supply for electrosynthesis. Connecting two cores with primaries in
series and rewinding a common center tap secondary over both cores produced very decent amperage (about 100A at 5V), but man was this setup bulky,
ineffective and in need of forced fan cooling. Long story short....investing into a decent switching power supply is the way to go if building the
power supply is not the primary objective of the experiment.
Exact science is a figment of imagination.......
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
I'm looking into building an arc furnace of my own. Does anyone know the resistance of a "typical" high current (8-10 A) arc? I would guess it would
be only a few ohms.
Edit: Upon further inspection, this question is ill-posed. Arcs take as much current as the ballast allows; the "resistance" (dV/dI) varies widely and
is often even negative.
What I really want to know is:
If I have a 120 VAC source and an inductive ballast with an impedance of 14 ohms (varies slightly with current due to nonlinear effects), what will
the current of the arc be?
[Edited on 9-10-2014 by Cheddite Cheese]
|
|
Dan Vizine
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 628
Registered: 4-4-2014
Location: Tonawanda, New York
Member Is Offline
Mood: High Resistance
|
|
If the current is determined by the ballast it would be about 8.6 amps, wouldn't it?
I've only recently started thinking about arc furnaces. Has anyone ever achieved practically useful results with anything less than a welder? It's
hard to see how, but I'm no expert.
[Edited on 10-10-2014 by Dan Vizine]
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
8.6 amps is assuming the ballast is the only impedance. However, I would assume the arc has some resistance, but it's probably pretty low.
Calculating: If the arc has a resistive impedance of 5 ohms (a high estimate), then that will bring the current down to 8.1 amps (never mind, this
difference will probably not matter).
|
|
macckone
Dispenser of practical lab wisdom
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2168
Registered: 1-3-2013
Location: Over a mile high
Member Is Offline
Mood: Electrical
|
|
For a good electric arc you need at least 2000 watts transformed to the arc with even higher being preferred. Industrial arcs are much higher
wattage.
|
|
markx
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline
Mood: Very Jolly
|
|
The resistance of the electrical arc has a negative dynamic profile...meaning as the current increases, the arc resistance decreases. Hence the
current limiting has to be done by the power supply. Either by an inductive choke, saturation of the transformer core (electrode welding transformers
use this option) or by switching supply current control.
Exact science is a figment of imagination.......
|
|
Metacelsus
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2537
Registered: 26-12-2012
Location: Boston, MA
Member Is Offline
Mood: Double, double, toil and trouble
|
|
Given the high power needs, I will probably reduce the impedance of my ballast. The highest current I can safely use is 15 amps. This should make my
power 1.8 kW (I'm using 120 VAC).
|
|
hyfalcon
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1003
Registered: 29-3-2012
Member Is Offline
Mood: No Mood
|
|
I know this is not exactly on topic but this old article has fascinated me since high school. Some day I'll get around to it.
http://books.google.com/books?id=YigDAAAAMBAJ&pg=PA100&a...
|
|
violet sin
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1477
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline
Mood: Good
|
|
that looks like a smaller article for the same thing I posted up a few. mine was from popular science as well. but gave directions for the balast
and 110v operation, but just said to use a couple crucibles or such. here it is again
http://blog.modernmechanix.com/mags/PopularScience/5-1933/ar...
" how to wind a simple coil reactance that controls the current, protects the fuses and cuts down greatly the cost of the electric power "
|
|
metalresearcher
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 737
Registered: 7-9-2010
Member Is Offline
Mood: Reactive
|
|
Well, a cheap ($100) hardware store welder of max 150A does work fine. For a bit more ($200) you can get a 150A inverter welder which provides DC. The
voltage is a safe value of at most 40V without load and 20V when running. Arcs running over 110V are unsafe.
I can make calcium carbide, melt (small quantities of) MgO, CaO and make Si from quartz sand and charcoal.
http://arcmelt.velp.info
|
|
violet sin
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1477
Registered: 2-9-2012
Location: Daydreaming of uraninite...
Member Is Offline
Mood: Good
|
|
well the way I see it, how much are you going to be processing is probably a big concern. if you just want to dork around with small amounts for the
experience and a bit of fun, it seems like the popular science version would be just fine. however, if you want to production run stuff, obviously a
welder would be the better call. I try to keep the devices I make smaller unless I need the big version specifically. storage space( especially),
funding and tools are pretty limiting factors for most.
small scale works just fine for me, as nothing I do makes money and I don't actually NEED to be doing it. technically I have to stay up late to just
have the spare time for projects. I just wish the reactance coil plans I found were written in number of turns, not overall dimensions of the
finished spool size. its not exactly common to find cotton braided shielding on enameled wire( much less hope it is the same diameter as in 1933. no
length was given, and no rating for the finished coil
|
|
Little_Ghost_again
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 985
Registered: 16-9-2014
Member Is Offline
Mood: Baffled
|
|
The best are arc welders with DC around 20V,cheap one with fans on the back cut out after a short time because of heat, but they produce upto 180A.
The way around the temperature problem is to build a non conductive enclosure, aim for around 30 litres in size, disconnect the fan and plonk the
whole thing in the vessel (set our current first). Fill the vessel with mineral oil.....REPEAT MINERAL OIL.............
It is non conductive, if you run the welder for more than 20 mins then add a pump and copper coil, place the coil in a bucket of water (or whatever)
connect one end to the top of vessel and the other end to the pump, then from the pump short bit of copper to the bottom of the vessel.
We have run our cheapo welder (for welding) for 5 years now and it happily welds for 2-3 hours (it might do more but I get bored after a couple of
hours welding lol)
|
|
Little_Ghost_again
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 985
Registered: 16-9-2014
Member Is Offline
Mood: Baffled
|
|
Forgot to add MOT are not safe to mess with, if your new to that kind of thing treat them like you would nitro glycerine or hydrofluoric acid, because
they take no prisoners and especially in the uk with 240V going in you dont get a second chance
|
|
Gooferking Science
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 97
Registered: 17-7-2013
Location: Somewhere in Kansas, USA...
Member Is Offline
Mood: Halogenated
|
|
Wow, a lot of great information on this thread. Thank you everyone for your input. Another method would be to buy a good ($200-$300) AC welder that
has an excellent duty cycle. One that can run near continously at ~100 amps. These are easy to find, and usually run on 240v. This could be rectified
to DC with some high current diodes and large capacitors. I think this would be a great power supply for an arc furnace.
A lincoln 225 amp "tombstone" welder has 20% duty cycle at max amperage. It would run for a long time at lower amperages.
[Edited on 23-12-2014 by Gooferking Science]
|
|
markx
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 645
Registered: 7-8-2003
Location: Northern kingdom
Member Is Offline
Mood: Very Jolly
|
|
Quote: Originally posted by Gooferking Science ![](images/xpblue/lastpost.gif) | Wow, a lot of great information on this thread. Thank you everyone for your input. Another method would be to buy a good ($200-$300) AC welder that
has an excellent duty cycle. One that can run near continously at ~100 amps. These are easy to find, and usually run on 240v. This could be rectified
to DC with some high current diodes and large capacitors. I think this would be a great power supply for an arc furnace.
A lincoln 225 amp "tombstone" welder has 20% duty cycle at max amperage. It would run for a long time at lower amperages.
[Edited on 23-12-2014 by Gooferking Science] |
Or the more contemporary solution fitting the 21st century....an inverter type welding apparatus. The cheaper ones go for about 150$ these days and
are quite appropriate for the task at hand.
If one has the desire to fiddle with the challenge of building one from scratch then some reference can be found here:
http://danyk.cz/svar_en.html
Although if the final objective is to run an arc furnace experiment I would not reccomend to go through the trouble of building the power supply for
it. It is really not worth the pain if one has no inclination towards the inner workings of power electronics.
Exact science is a figment of imagination.......
|
|
Endo
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 124
Registered: 5-1-2006
Location: USA
Member Is Offline
Mood: Cold
|
|
A friend and I are working at building a carbon arc furnace like the one shown in this video: https://youtu.be/VTzKIs19eZE
We got a couple of free microwaves and removed the useful stuff, including two transformers. I have a couple questions about how to best balance the
transformers when rewinding them. The two transformers are from different wattage ovens, I intend to hook them up in series and am unsure what the
ultimate output goal should be. Do I want to just balance the output voltages to be the same or should I attempt to balance (VA) to minimize the load
differences causing one transformer to overheat sooner? I have removed the secondary (HV windings) from both transformers and re-wrapped the cores
with #8 gauge wire. I have wrapped the smaller transformer with the maximum number of wraps I can fit (15turns). The larger transformer can take
more wraps, (12.5 wraps outputs the same voltage as the smaller transformer, although I could fit several more if needful)
With these in series should I leave the heavier transformer with less wraps or add as many as I can fit?
detail on the the transformers are as follows:
Small transformer: Primary Resistance 0.7 Ohms, Secondary 15 wraps, 0.3 Ohms, voltage output 14.6v. (120V in)
Larger Transformer: Primary resistance 0.4 Ohms, Secondary 12.5 - ? wraps, voltage output 14.6v to ~20v.
Thanks
|
|
WGTR
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 971
Registered: 29-9-2013
Location: Online
Member Is Offline
Mood: Outline
|
|
If the secondaries are connected in series, they will have the same current going through both of them at the same time. Calculate the number of
turns such that each respective core stays within its VA ratings at the expected load current. The voltage output for the smaller core will be less
than the larger one in this case. Wire gauge size may need to increase or decrease depending upon the given number of turns needed.
My $0.02.
Also, I think you'll find the arc to be a bit unstable with a 30-40V supply, due to the arc's strong negative resistance characteristic. It will want
to go between the two extremes of pulling too much current, or not enough to keep the arc going. Graphite electrodes do allow for a stabler arc than
other materials, however.
I think you'll have better success with a 60-80V output, with a large ballast resistor or inductor in series to help stabilize the current. It's like
calculating the series resistor to bias an LED. The arc voltage will probably run between 15-30V, depending on current. That leaves 30-65V across
the resistor/reactor. Using Ohm's Law will allow you to calculate the needed ballast for a given range of amperage.
[Edited on 10-23-2015 by WGTR]
|
|