Sintering Fe3O4 powder?
I've given some thought on sintering Fe3O4 powder using induction heating to obtain a solid chunk/rod/weird shape of magnetite to use as a
chlorate anode. The idea struck me when seeing this: http://www.powerlabs.org/indheating.htm
Does anyone have any spontaneous ideas?
|
|
chloric1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1089
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
Microwave Responsive
If you maybe put a beaker of 1000 ml of water in a microwave to protect the magnetron and then simply put your magnetite in the microwave it should
get quite hot. Actually, I have a few microwave chemistry articles. One actually depicts a mold cavity with silicon carbide coating inside as heating
element. An ideal setup like this should reach 1500 C.
What could be used as a binder for magnetite. It is an oxidizer easily reduced by carbon compounds.
Fellow molecular manipulator
|
|
Twospoons
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1309
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline
Mood: A trace of hope...
|
|
What size particles? How big a chunk do you want?
My gut feeling is that microwave is too high a frequency to get the penetration you'll want. You'll plenty of heating in the first
centimetre or so, but very little in the centre.
Energy penetration will improve as the frequency drops, but absorption drops too ( to zero at DC, obviously).
Gut feel again - I'd go for something in the 500kHz to 1MHz region. Building a high power FET bridge for those frequencies shouldn't be
impossible - neither will it be easy, since you're going to want 500 - 1000 W output.
Maybe a resonant bridge?
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
How about using ye big furnace?
I haven't researched much about the melting point of Fe3O4, but I have gotten some to fuse onto clay in my furnace and make a glaze. (Of course
some parts turned red - Fe2O3 becuase the furnace atmosphere isn't controlled)
And this works for chlorate? In place of lead dioxide? That would just be way too simple! Next time I fire my furnace I might throw in a bit of
Fe3O4 in a clay crucible and see how it goes.
|
|
chloric1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1089
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
Needs a binder or high pressure for shapes
Since most binders would reduce magnetite at high temps then a hydraulic press capable of 2000 or 300 psi would work follwoing by an oxidizing
atmosphere. A few centimeters would work for small rods. The problem is the magnetite would have to be pretty dense for effective conductivity.
Two spoons, what references would you recoomend concerning 500W or 1000W resonant bridges? It could be interesting and I would surely like to learn
more. I do have basic electronic knowledge.
Fellow molecular manipulator
|
|
rift valley
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 103
Registered: 24-7-2004
Location: NH
Member Is Offline
Mood: semiconducting
|
|
My Merck Index is tells me that magnetite has a melting point of 1538C. It also says that it oxidizes to Iron (III) oxide when heated in the presence
of air.
|
|
Twospoons
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1309
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline
Mood: A trace of hope...
|
|
chloric1: I don't have specific refs, but browsing the Application Notes from the major semiconductor manufacturers can be very rewarding. For
power electronics look at comps like International Rectifier, National Semiconductor, OnSemi, TI, IXYS, Harris, Infineon, Fairchild, Philips
Semiconductor, SGS Thompson ... There's a wealth of info out there - just got to hunt for it!
These Ferrite electrodes from TDK might be useful.
[Edited on 2-2-2005 by Twospoons]
|
|
Chris The Great
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 463
Registered: 29-10-2004
Location: Canada
Member Is Offline
Mood: No Mood
|
|
I dunno, I'd just slap it into the microwave without any water and turn it on, and stop when it's done. I'd be more concerned about
the stuff spilling onto the microwave, or the electronics getting to hot from the amount of heat present.
Also, if you do use a microwave, get and old 1500W one. Not only will you get enough power to actually DO stuff, you won't be able to kill it.
Trust me on that one And I've put some weird things in microwaves,
including, but not limited to: Boiling down battery acid, 60W light bulbs (mini lighthouse), 40 gauge wire (plasma!), computers, etc.
Just make sure that the heat radiated by it as it heats up to 1500C doesn't get onto the sides of the microwave, as it may overheat the
electronics and melt the plastic parts.
You might also be able to turn an u-wave into an arc furnace.....just though of that. Hmm, planning needs to be done. An arc furnace with a u-wave
field. Now that's my kinda project! Would take a fair amount of work though.
|
|
chloric1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1089
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
Quote: | Originally posted by Twospoons
chloric1: I don't have specific refs, but browsing the Application Notes from the major semiconductor manufacturers can be very rewarding. For
power electronics look at comps like International Rectifier, National Semiconductor, OnSemi, TI, IXYS, Harris, Infineon, Fairchild, Philips
Semiconductor, SGS Thompson ... There's a wealth of info out there - just got to hunt for it!
Oh yes! I forgot about the spec sheets! If I got desperate I am sure I could
call for engineering support or send email. This relatively moderate frequency would also be good for speeding up dissolution of difficultly soluble
ingredients or making more homegenous slurries.
These Ferrite electrodes from TDK might be useful.
P.S Thnak for the link, I will have to contact TDK and ask for minimum orders and such. I just tell them I have a 40000 gallon pool I need to
chlorinate![:cool:](./images/smilies/cool.gif)
[Edited on 2-2-2005 by Twospoons] |
[Edited on 2/2/2005 by chloric1]
Fellow molecular manipulator
|
|
Twospoons
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1309
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline
Mood: A trace of hope...
|
|
Do I detect a hint of sarcasm over the TDK link? Seems you have yet to explore the wonderful world of FREE SAMPLES. Its a totally brilliant scam
I've often used to obtain parts - cook up a project, pretend to be a company and request some samples. Usually you'll get them couried to
you gratis. Occaisionally you'll get a "no", or need to pay for the samples( but its still better than 10,000 pc MOQ !). From the
suppliers point of view the few bogus requests are not worth worrying about - its small potatoes compared the the business they can acquire by sending
samples to genuine customers. I'm currently building a home theatre amp from free parts from TI and Nat Semi.
Hey Chris_the_Great: uWave arc has been done! Google search will turn up lots of ideas to play with. Generally requires a tapered waveguide, shorted
at the ends. The arc forms ~1/4 wave from the short, at the narrow end. Its also useful to have some tuning stubs somewhere in the waveguide, and a
circulator feeding a dummy load so any residual power doesn't wind up back in the magnetron.
[Edited on 2-2-2005 by Twospoons]
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
Ok, if the mp is 1538 deg. C, then I think I can get temperatures good enough to sinter it at least, but that's just my guess.
Yeah, it would oxidize in air, but with a working oil burner and charcoal, I think I, or others, can pretty near a neutral atmosphere.
Chris, you could also use the transformer in the microwave and another transformer as an inductor, and make a more standard arc furnace, which I hope
to do. (got the transformers) That'll need some crazy refractories, but I have a crazy idea- bake a cake and burn it on purpose- this cake would
have zircon, or magnesia in it, and now we have a magnesia carbon bonded refractory. I've gotta try it.
Yes, I'm still working on refractories, and BromicAcid, I will have a paper on refractories that I'll post here by the end of April.
|
|
Twospoons
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1309
Registered: 26-7-2004
Location: Middle Earth
Member Is Offline
Mood: A trace of hope...
|
|
Maybe its a silly idea, but maybe the magnetite powder could be fed into an oxy/propane torch, like the way ruby laser rods were made by feeding doped
alumina into an H2 /02 torch. The molten particles exiting the flame are aimed at a rotating substrate, and as the torch is slowly withdrawn the fused
material builds into a long rod.
|
|
Mumbles
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 436
Registered: 12-3-2003
Location: US
Member Is Offline
Mood: Procrastinating
|
|
Instead of sintering preexisting Mangenite, why not try to make the mangenite which would fuse into a mass?
I'm thinking 1 molar part Ferrous sulfate, and 1 molar part Ferric sulfate mixed in excess with NaOH. Heat to probably 5-600C and it will
convert to mangenite. Washings with water will remove unreacted Iron Sulfates and Sodium sulfates. It may actually form a porus block that has a
decent surface area.
What about just pressing the mangenite using some sort of non-polar binder?
|
|
Chris The Great
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 463
Registered: 29-10-2004
Location: Canada
Member Is Offline
Mood: No Mood
|
|
Hmm, some time ago I started building a Mega Microwave, which would have a water cooled magnetron running at over 10,000 watts AC input. I
didn't finish as I didn't have anything I could make the hose connect to the magnetron in a watertight manner. But it might be something I
may take up again.
I only need to make the water cooling part, and fix my busted 240V circuit to power it.
Actually, maybe I'll just forget the cooling, and turn it off when the magnetron glows red
|
|
chloric1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1089
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
HEHHE
THats right Chris the great! Live dangerously!![:D](./images/smilies/biggrin.gif) ![:D](./images/smilies/biggrin.gif)
[Edited on 2/3/2005 by chloric1]
Fellow molecular manipulator
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
I can use a 2 ton tile press at the local ceramic place for like $4 an hour, so that might be an option to make electrodes.
I'll do some tests.
|
|
chloric1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1089
Registered: 8-10-2003
Location: GroupVII of the periodic table
Member Is Offline
Mood: Stoichiometrically Balanced
|
|
Quote: | Originally posted by Twospoons
Do I detect a hint of sarcasm over the TDK link?
[Edited on 2-2-2005 by Twospoons] |
I did not mean anything by it. The free sample route may be some aproach I could take. I could stick with my 40000 gal pool story or maybe I am a
motorcycle customizer and I need them for chrome plating. I definately wont be buying 10000 electrodes anytime soon. My car is in the shop and my
daughter is do to be born this month!!![:o](./images/smilies/shocked.gif) I need to hoard my cash!
Fellow molecular manipulator
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
Sintering Fe3O4
Well I heated black iron oxide from the pottery store (I'm pretty sure it's magnetite) in a crucible in the furnace, and it sintered/melted
quite nicely into a solid mass at the bottom. No problems there. It did of course oxidize a bit- it is now greyish and in some places red. I'm
confident that the oxidation itself is no big deal- a covered crucible would help, and so would a covering of flux (NaCl and CaCl2 or something else
with a reasonably low melting point) The starting iron oxide and the end product were both magnetic, though the sintered powder was much less
magnetic.
The problem is that none of the iron oxide (fired or not fired) is electrically conductive! (as far as I can tell with my pathetic analog meter) How conductive ought these electrodes to be?
Maybe I should do some tests to make sure I really do have magnetite.
In conclusion, I don't think binders are really nescessary, but if ya want them maybe something like a low melting temperature glass (high
fluxes) or sodium silicate would be suitable.
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
Sorry to double post and all, but did we ever find out if Fe3O4 is electrically conductive? This might be an important consideration if it is to be
used as an electrode. Otherwise I like this process a lot. I can sinter my "black iron oxide" which is magnetic pretty easily in my
furnace. The m.p. of Fe3O4 is 1420 deg. C. though, and I didn't think my furnace got that hot on that run.
|
|
12AX7
Post Harlot
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
Sintering works a lot lower than the melting point, although best results (without hot pressing) do come just below.
You might try another metal oxide, say litharge, to liquid phase sinter it. Well, maybe something a little more/less reactive, since the ultimate
goal is what, perchlorate cell?
Tim
|
|
Cyrus
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 397
Registered: 24-4-2004
Location: Ancient Persia
Member Is Offline
Mood: No Mood
|
|
Yeah, perchlorate cell, why not? ![:)](./images/smilies/smile.gif)
I don't know about litharge, but PbO2 decomposes, right? So that won't work as far as sintering goes...
The iron oxide really looked kind of melted- it shrunk to about 1/3 of its original size... would sintering do that?
|
|
12AX7
Post Harlot
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline
Mood: informative
|
|
Yeah- but 1/3? Is that 33 or 66% shrinkage? Even for a coarse grain,
that's an awful lot of shrinkage.