Silver Mirror Coated Glassware
Hello fellow Mad scientists today I have succesfully done a silver mirror coating on the inside of a 1000ml RBF and figured I'd share some of the
difficulties and a couple pictures of the outcome as I did not find any guides on this website already. Nurdrage has a pretty decent video on youtube
for anyone interested in a step by step visual guide.
Here is a picture of the finished product ![:D](./images/smilies/biggrin.gif)
![IMG_1135.jpg - 74kB](http://www.sciencemadness.org/talk/files.php?pid=302290&aid=26558)
The procedure I used, it is based on a MIT lab that Ill upload at the end of this post. I found this lab to be very well written and all the credit
goes to its author. As for the difficulties I mentioned there were only two.
The first problem I ran into is that the initial coating was not very thick and was hardly reflective at all, this was overcome by repeating the
process of mixing all 3 mirroring solutions in the flask twice versus once. Heres a picture showing the lack of coating.
![IMG_1124.jpg - 52kB](http://www.sciencemadness.org/talk/files.php?pid=302290&aid=26560)
Another issue I had was that all the precipitate formed after the solutions were mixed formed a big mud ball like blob and scratched the initial
mirror coating quite a bit, this was fixed EXTREMELY carefully rotating the flask not allowing the blob to get stuck in one place as well as using a
second go with the mirroring solutions. Heres a picture showing some of the scratches mentioned.
![IMG_1125.jpg - 42kB](http://www.sciencemadness.org/talk/files.php?pid=302290&aid=26562)
And a final note is that you need to wash whatever it is youre coating extremely throughly or the silver will not stick well. For me I initially
washed the flask with soap water until no bubbles formed when more tap water was added, then added acetone and swished around the flask for about 2
minutes, then I drained the flask and washed 3 times with some distilled water. That cleaning has produced very good results for me if anyone has any
recommendations for cleanings more suited for this procedure please do share!
The purpose of why I am doing this is I plan on doing some dry distillations that use sodium hydroxide so I wanted to see if this mirror coating will
negate the damage that would normally occur to the glassware I'll share the results as soon as I'm done with that project. I originally saw this idea
listed in the benzene production thread and figured I'd try it. If anyone has already tried using a mirror coating to protect your glassware please
let me know if it didnt work so I can save a flask!
And heres how to make the solutions listed in the lab so you dont have to math ![:D](./images/smilies/biggrin.gif)
1.5M NH4NO3
100mL H2O + 8g NH4NO3
250mL H2O + 20g NH4NO3
2.5M NaOH
100mL H2O + 10g NaOH
250mL H2O + 25g NaOH
.5M AgNO3
100mL H2O + 8.5g AgNO3
250mL H2O + 21.25g AgNO3
5% Dextrose
100mL H2O + 5g Dextrose
250mL H2O + 12.5g Dextrose
Attachment: Silver mirror coating.pdf (316kB) This file has been downloaded 470 times
[Edited on 6-10-2013 by PeeWee2000]
“Everything is relative in this world, where change alone endures.”
― Leon Trotsky
|
|
frenchemist1
Harmless
Posts: 5
Registered: 6-6-2013
Member Is Offline
Mood: No Mood
|
|
As an evidence, silver metal would be easily removed with nitric acid... Of course !
|
|
elementcollector1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline
Mood: Molten
|
|
I'm interested to see if this works out - I'd love to be able to boil NaOH solutions down in regular glassware.
Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
|
|
Pyro
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1305
Registered: 6-4-2012
Location: Gent, Belgium
Member Is Offline
Mood: No Mood
|
|
I don't think a silver layer that thin will work.
you can scratch it off with your nail if it isn't perfectly coated
all above information is intellectual property of Pyro. ![:D](./images/smilies/biggrin.gif)
|
|
bismuthate
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 803
Registered: 28-9-2013
Location: the island of stability
Member Is Offline
Mood: self reacting
|
|
That would an accident just waiting to happen. One scratch in the silver and you will have hot NaOH all over.
|
|
elementcollector1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline
Mood: Molten
|
|
Could always plate the silver with something stronger, maybe a thick coating of copper?
Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
|
|
bismuthate
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 803
Registered: 28-9-2013
Location: the island of stability
Member Is Offline
Mood: self reacting
|
|
That would work but how do you copperplate glass?
|
|
elementcollector1
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2684
Registered: 28-12-2011
Location: The Known Universe
Member Is Offline
Mood: Molten
|
|
Well, it's silver-plated already, so it's electrically conductive.
Elements Collected:52/87
Latest Acquired: Cl
Next in Line: Nd
|
|
bismuthate
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 803
Registered: 28-9-2013
Location: the island of stability
Member Is Offline
Mood: self reacting
|
|
Good point. I didn't think of that this could open up so many possibilities for me becase I have no metal comtainers but, I do have AgNO3.
|
|
PeeWee2000
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 58
Registered: 2-7-2013
Location: Michigan
Member Is Offline
Mood: No Mood
|
|
Well I know its fairly thin but I'm hoping that as long as I am gentle when pouring the chemicals in that it shouldn't damage the coating but this may
just be wishful thinking, also I plan on silver coating my condenser and recieving flask too as the distillate is corrosive to glass as well not
nearly as much as NaOH though. I'll know soon enough though and the reaction should be proceeding at temperatures well under 100C so hopefully I wont
have a hot mess of hot NaOH all over I might do a trial run this weekend I'll
be sure to let you all know how it goes if I do
“Everything is relative in this world, where change alone endures.”
― Leon Trotsky
|
|
Dariusrussell
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 70
Registered: 27-6-2013
Location: Southie
Member Is Offline
Mood: Organometallics
|
|
I definitely second electroplating the silver, or at least adding a few more layers before doing a trial. Its concerning that you can see through the
silver coating in places and etched glass isn't all that great.
|
|
PeeWee2000
Hazard to Self
![*](images/xpblue/star.gif)
Posts: 58
Registered: 2-7-2013
Location: Michigan
Member Is Offline
Mood: No Mood
|
|
I already have added another layer and light cannot pass through the silver layer anymore and there are no more visible scratches the second and third
pictures were before I added a second layer. But indeed being able to see through it was concerning which is exactly why I added another coating ![:D](./images/smilies/biggrin.gif)
And as for electroplating I'd like to but it wouldn't be the easiest to do being inside the flask and I don't have any readily available copper
plating solutions or the tools to do so.
[Edited on 12-10-2013 by PeeWee2000]
“Everything is relative in this world, where change alone endures.”
― Leon Trotsky
|
|
bfesser
Resident Wikipedian
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2114
Registered: 29-1-2008
Member Is Offline
Mood: No Mood
|
|
I thought I had posted this a couple days ago, but I guess it slipped my mind. In my topical compendium (link in sig), under <a
href="viewthread.php?tid=25000#copper">copper</a>, there are links to a couple topics of interest.
<strong><a href="viewthread.php?tid=21268">OTC Copper Mirror</a></strong>
(I recall seeing another Cu mirror topic, but can't seem to find it at the moment.)
|
|
bismuthate
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 803
Registered: 28-9-2013
Location: the island of stability
Member Is Offline
Mood: self reacting
|
|
I found a video on making silver mirrors here.
http://www.youtube.com/watch?v=6vduHWV47Dg
This channel is pretty good in my opinion.
|
|