MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 16-1-2013 at 10:09
Acid Etching Metals


I have a little Valentine's Day project I'm working on that I had a question about, if anyone is familiar with acid etching the surface of metals. I've seen videos and pictures of the "bismuth heart" and that's what I'm trying to recreate.



Video example here: http://www.youtube.com/watch?v=W7PpIVi-U6k

To reveal the crystal regions, the surface is etched with an acid for a short period. Does anyone have any recommendations for a good acid solution to do such etching? Type of acid, strength, etc. I've tried hardware store hydrochloric on bismuth and tin metals with decent results, but I was wondering if there was an acid better suited to this. I'm making my heart out of tin because of its lighter weight.

I did a little googling and a few places recommended a combination of HF and HNO3. I'd prefer not to work with HF if I can avoid it (I do have ammonium bifluoride), so perhaps nitric alone would yield acceptable results?
View user's profile Visit user's homepage View All Posts By User
AJKOER
Radically Dubious
*****




Posts: 3026
Registered: 7-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 16-1-2013 at 10:39


HCl/H2O2 is an etching solution, which you may give a try.

View user's profile View All Posts By User
Poppy
Hazard to Others
***




Posts: 294
Registered: 3-11-2011
Member Is Offline

Mood: † chemical zombie

[*] posted on 16-1-2013 at 10:48


In crystallography, etch figures appears as result of slow dissolution of the crystal interface from Crystals and Crystal Growth, buy Alan Holden and Phylis Morrison, pg. 261
Corrosion with acids is commonly accompanied by the release of hydrogen in the form of bubles, which can mess the shape of the striations. Fo that you can use a mix of acid and sodium chlorate, whereas the chlorate acts as an accelerator preventing the release of hydrogen in the atack site, much as the HCl/ H2O2 mix.
Use very weak concentrations.

[Edited on 1-16-2013 by Poppy]
View user's profile View All Posts By User
bfesser
Resident Wikipedian
*****




Posts: 2114
Registered: 29-1-2008
Member Is Offline

Mood: No Mood

[*] posted on 16-1-2013 at 10:52


I unintentionally did this with a lump of Zn once. If memory serves, it was in aqueous ethylenediaminetetraacetic acid (EDTA). It was beautiful. EDTA may work on Sn.



View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 17-1-2013 at 11:35


Thanks for the tips, all! The acid/chlorate mix is an interesting suggestion - what's the equation for such a reaction (i.e. where does the hydrogen go)? I have some potassium chlorate that I'll try out in combination with HCl.

EDTA is another possibility, but can that be had OTC? Googling EDTA returns mostly health and nutrition type products, which I wouldn't want to go through the trouble of extracting if at all possible.

I think so far the two most promising experiments will be HCl/chlorate and nitric acid, all in dilute solution. I'll do some testing this weekend.
View user's profile Visit user's homepage View All Posts By User
mnick12
Hazard to Others
***




Posts: 404
Registered: 30-12-2009
Location: In the lab w/ Dr. Evil
Member Is Offline

Mood: devious

[*] posted on 17-1-2013 at 11:48


I worked in a lab where we did a lot of etching for examination of micro-structures. We were mostly looking at carbon steels, and for this purpose we used a common etchant called nitol. Which is composed of 3-5% nitric acid in reagent alcohol. This work wonderfully for exposing the carbide distribution in steel, but it was not effective for the more corrosion resistant alloys.

For the super alloys (A286 mostly) we used a solution of copper sulfate in concentrated hydrochloric acid, this forms the really pretty chlorocuprate ions. This stuff is really strong and can easily over etch many metals. I would suggest you start out with very dilute enchants, and work your way up until you find something that works for you.

It is very easy to over-etch stuff, stronger is not always better.
View user's profile View All Posts By User
chemrox
International Hazard
*****




Posts: 2961
Registered: 18-1-2007
Location: UTM
Member Is Offline

Mood: LaGrangian

[*] posted on 18-1-2013 at 01:10


Also talk to a machine shop or two about "pickling" solutions.



"When you let the dumbasses vote you end up with populism followed by autocracy and getting back is a bitch." Plato (sort of)
View user's profile View All Posts By User
phlogiston
International Hazard
*****




Posts: 1378
Registered: 26-4-2008
Location: Neon Thorium Erbium Lanthanum Neodymium Sulphur
Member Is Offline

Mood: pyrophoric

[*] posted on 18-1-2013 at 07:45


In addition to the mentioned etchants, you might try ferric chloride or ammonium persulfate, both used for etching electronic circuit boards and readily available OTC for this purpose.

Do be careful with chlorate+acid!
The ClO2 gas released is explosive and poisonous. Check Woelens page for some actual experiments with this gas.

Why is it actually that these crystal faces become so clearly visible upon etching while you don't really see them if you simply cut and polish a metal?

[Edited on 18-1-2013 by phlogiston]




-----
"If a rocket goes up, who cares where it comes down, that's not my concern said Wernher von Braun" - Tom Lehrer
View user's profile View All Posts By User
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 18-1-2013 at 08:26


phlogiston:

EEk! You're right about ClO2: chlorate + acid + reducing agent = chlorine dioxide. The metal being etched acting as the reducing agent. If I keep everything very dilute, though, I think things should go smoothly. Just in case, I'll try this one outside in a wide container to avoid confining any gas produced.
View user's profile Visit user's homepage View All Posts By User
12AX7
Post Harlot
*****




Posts: 4803
Registered: 8-3-2005
Location: oscillating
Member Is Offline

Mood: informative

[*] posted on 18-1-2013 at 11:34


I've used HCl + CuCl2 + NaClO3 numerous times for etching circuit boards. The chlorate must be added incrementally, only as needed. The copper chloride serves as a redox reservoir, dissolving metal and forming Cu(I), which, with the Cu(II) and excess of chloride, forms an intensely dark brown complex. Chlorate is instantly decomposed to Cl2 under these conditions, which further reacts with the Cu(I), turning the solution transparent green once again. Never add more than the amount required to clarify the solution at any given time, as an excess results in bubbles of Cl2. (A really fast addition probably would result in ClO2, so don't do that, either!)

Etch rate isn't too rapid, I'd guess I'd spend half an hour etching a 1 oz. board (0.0014" / 35um copper) at 60-80C. Agitation and bubbling help greatly.

Tim




Seven Transistor Labs LLC http://seventransistorlabs.com/
Electronic Design, from Concept to Layout.
Need engineering assistance? Drop me a message!
View user's profile Visit user's homepage View All Posts By User This user has MSN Messenger
MrHomeScientist
International Hazard
*****




Posts: 1806
Registered: 24-10-2010
Location: Flerovium
Member Is Offline

Mood: No Mood

[*] posted on 22-1-2013 at 07:14


I did some experimenting this weekend, and here are my notes.

Acids:
9.5M HCl (hardware store grade)
16M HNO<sub>3</sub>

Metals: Sn, Bi - each melted and cast into a graphite heart-shaped mold & allowed to cool slowly

I tried a number of different etching baths; each starting with 18mL distilled water and adding 1 - 3mL of acid to each. These amounts were governed by the size of the small Petri dishes I used. Thus,
Bath #1 = 18mL H2O + 1mL HCl
Bath #2 = 18mL H2O + 2mL HCl
Bath #3 = 18mL H2O + 3mL HCl
Bath #4 = 18mL H2O + 1mL HNO3
Bath #5 = 18mL H2O + 2mL HNO3
Bath #6 = 18mL H2O + 3mL HNO3

I placed each metal in each bath for roughly 20 minutes. I stopped after this long because of the comment in the video in my original post, where he claims his etching took place after only a "few minutes". The only solutions that had any visible impact on the bismuth were #3 and #6, the most concentrated. These only revealed a very faint crystal structure; nowhere near the sparkle of the picture I showed above and not good enough for my purposes.

The more interesting result was tin. It showed no change at all in HCl, but even the very low concentration of nitric acid quickly formed a black film on its surface. I left both metals in Bath #3 for about an hour, just to see what happened, and there was slight etching on the Bi and no change to Sn. Adding just a few drops of one of the dilute nitric baths to this one caused the black coating to develop on the tin within only a few minutes. It can be buffed off, but no etching has occurred.

I tried etching of bismuth with HCl a long time ago, and if I remember right I diluted the acid to 50% its original strength (equal parts water & acid). This gave decent results, so maybe I'll try something closer to that in my next set of trials. What's interesting is it looks like nitric acid of any concentration is unsuitable for etching tin in the way I want (it may yet work for Bi, if I increase the concentration).