Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
Purifying Zn powder from alkaline batteries' Zn paste
Hi everyone, i've got some zinc paste from alkaline batteries (it should be zinc powder, but i'm not sure. That's basically the problem) and
i was looking for a way to purify it.
It still has all of the electrolytes in it (some of which also exothermically reacted when they came in contact, probably i shouldn't have mixed
different batteries) and also a bit of water that accidentally got inside while i was cooling down the container from said reaction.
One of the biggest problems is that i don't even know for sure wether it's zinc powder or some sort of salt, because it looks way too white-ish to me
to be zinc powder, but that maybe from the electrolytes, i don't know.
I made a video of the paste but, ironically, speaking of batteries i can't find my camera's battery and i had to record it with the phone...
Sorry for the crappy quality and also for my horrible accent, lol.
The vid is here: http://www.youtube.com/watch?v=crEN0-uT-TQ
|
|
Endimion17
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline
Mood: speeding through time at the rate of 1 second per second
|
|
Just wash it quickly to avoid it being consumed by the dissolved base, and then heat a small amount until it oxidizes. It burns with bluish flame,
evolving lots of zinc oxide smoke.
Its oxide is yellow when it's hot, and white when it's cold.
If the batteries were old, not much zinc will remain...
You sound like a Enrico Fermi crossed with Super Mario. That's cool.
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Any zinc in there will have been used up: i.e. irrecoverably oxidised.
If Zn metal is what you're looking for then look to the zinc sheet casings of these batteries.
BTW, it takes more than 'washing' to get to the MnO2 in battery crud. The manganese oxides in there are mixed with graphite and other stuff. Search
the forum for a multitude of threads on extracting manganese from battery crud.
|
|
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
Lol Fermi mixed with Super Mario, who knew that ![:D](./images/smilies/biggrin.gif)
Ok so i washed the solution and it's now filtering (it will take at least 1 hour i think, i used a regular paper sheet and not filter paper which i
don't have).
After it finishes i'll wash it again and do the rest tomorrow.
For the heating, should i do it with free flame or on a plate?
|
|
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
Sorry, you replied while i was replying too and i didn't see it.
Yeah, seems to turn out you're right - although it's not dried up yet (i rewashed it and it's now re-filtering) the powder appears to be white oxide.
I was looking for the powder, i know i can get zinc from the casings (but only carbon-zinc casings, alkaline cases are actually made of cheaper
steel).
For the MnO2, i found out that graphite usually floats on water, and slowly overflowing the beaker with water makes it drip out of it while leaving
the MnO2 on the bottom.
As a further test, i tried igniting the powder with an oxidizing flame and nothing happened, so i'm quite sure it is only MnO2.
|
|
simba
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 175
Registered: 20-5-2011
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Demonblack ![](images/xpblue/lastpost.gif) |
Ok so i washed the solution and it's now filtering (it will take at least 1 hour i think, i used a regular paper sheet and not filter paper which i
don't have).
|
Is it so hard to get at least a coffee filter? With the time you used to wait it to filter, you could have used to go buy some instead.
|
|
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
It was 23:30 here when i started the filtering...
[Edited on 24-11-2011 by Demonblack]
|
|
simba
Hazard to Others
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 175
Registered: 20-5-2011
Member Is Offline
Mood: No Mood
|
|
Oh well...I guess not everyone is a coffee addict like me, I think I have more filter paper then sulfite in my house.
|
|
Sedit
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1939
Registered: 23-11-2008
Member Is Offline
Mood: Manic Expressive
|
|
If you need Zinc and can't think of any other source then take as many US pennies as you can and put them in a pan on the stove. Before you know it
the Zinc will melt out and you will be able to pour off, with ease, a mess load of relatively pure Zinc.
Pennies are cheep and the newer the US penny, the more Zinc they contain. What a wonderful economy we live in when our coins are worth only a small
fraction of there real value.
Knowledge is useless to useless people...
"I see a lot of patterns in our behavior as a nation that parallel a lot of other historical processes. The fall of Rome, the fall of Germany — the
fall of the ruling country, the people who think they can do whatever they want without anybody else's consent. I've seen this story
before."~Maynard James Keenan
|
|
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
I don't live in the US, so pennies aren't an option...
What about euro cents?
I also saw on youtube a video in which the maker used some roof thing made of zinc, they sell it in stripes to prevent corrosion or something. Might
be a good source.
By the way having the Zinc and having it in powder is not the same lol.
Is there any simple way to reduce the oxide i got and still get a powder (-> no thermite)?
|
|
Endimion17
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline
Mood: speeding through time at the rate of 1 second per second
|
|
If you live by the sea and there's a shipyard nearby (or any place where people repair their boats), go there and ask them to give you their waste
zinc anodes. Those things are fairly large, porous and covered with zinc oxide, sodium chloride and small marine life so you'll have a hard time
getting the pure metal, but it's worth it.
Be sure to ask for zinc, because they might give you aluminium.
I'm not sure that roof thing is zinc. It's probably zinc plated steel, common and usually worthless junk to home chemists.
Otherwise just buy the anodes. Zinc is not expensive.
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Endimion17 ![](images/xpblue/lastpost.gif) | I'm not sure that roof thing is zinc. It's probably zinc plated steel, common and usually worthless junk to home chemists.
|
You can buy zinc cladding here, for roofing jobs etc. This is soft anf malleable and mainly zinc, a little alloyed probably.
But what's wrong with the zinc casings from Zn/MnO2 batteries? Granted, it's not powder...
Quote: Originally posted by Demonblack ![](images/xpblue/lastpost.gif) | For the MnO2, i found out that graphite usually floats on water, and slowly overflowing the beaker with water makes it drip out of it while leaving
the MnO2 on the bottom.
As a further test, i tried igniting the powder with an oxidizing flame and nothing happened, so i'm quite sure it is only MnO2.
|
To remove all the graphite by floatation only is nigh impossible IMHO: the two materials are far too much interwined for that, it's a real
paste, not just a dry blend of two powders. Just trying to ignite your powder is a poor test. Dissolve some in HCl: you’ll be left with at least
some black residue of graphite (the liquid phase contains the Mn as MnCl2). The subject of extracting the manganese oxides from battery crud has been
exhausted to destruction here on this forum in various often lengthy threads.
[Edited on 25-11-2011 by blogfast25]
|
|
S.C. Wack
bibliomaster
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 2419
Registered: 7-5-2004
Location: Cornworld, Central USA
Member Is Offline
Mood: Enhanced
|
|
It is not challenging to get a nice shiny powder from alkalines. It may be impossible from some brands, but is very easy from others (once you've got
the case open).
|
|
woelen
|
Thread Pruned 28-11-2011 at 00:02 |
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
Sorry for the absence.
What's wrong with them? That i don't have tons of carbon-zinc batteries, lol
Quote: Originally posted by S.C. Wack ![](images/xpblue/lastpost.gif) | It is not challenging to get a nice shiny powder from alkalines. It may be impossible from some brands, but is very easy from others (once you've got
the case open). |
I suspect i didn't get any zinc because i used depleted batteries (the best-performing one putting out 0.23 amps shorted).
I should try with a new battery, but even if that works it's kind of wasteful.
By the way, i think i got ZnO.
It's a very fine powder (there are some bigger clumps but just because i didn't break them well enough), light gray, somewhat tending to blueish.
|
|
Endimion17
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 1468
Registered: 17-7-2011
Location: shores of a solar sea
Member Is Offline
Mood: speeding through time at the rate of 1 second per second
|
|
Nothing is wrong. It's just very expensive, compared to waste anodes. I've managed to get mine for free. It's essentially waste.
It was big as a 1 liter bottle, meaning several kilograms in mass, and all it took was a few nice words with the kind worker at the shipyard.
Purifying it was a nightmare. It took me a whole afternoon of messing with refractory bricks, tongs and propane-butane fire to deliver enough heat to
the huge anode. The temperature is not a problem, but the heat... holy cow. ![:o](./images/smilies/shocked.gif)
I don't have large enough crucibles, nor a furnace, so I had to heat the whole anode several times, filling my steel crucible beneath.
I was outside the ventilated room most of the time, but even with that precautions, I've even managed to get slight "zinc shakes" simply because it
took so long. 24h later I was OK.
Ah, good times. ![:D](./images/smilies/biggrin.gif)
[Edited on 4-12-2011 by Endimion17]
|
|
blogfast25
International Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Endimion17 ![](images/xpblue/lastpost.gif) | Nothing is wrong. It's just very expensive, compared to waste anodes. I've managed to get mine for free. It's essentially waste.
It was big as a 1 liter bottle, meaning several kilograms in mass, and all it took was a few nice words with the kind worker at the shipyard.[Edited
on 4-12-2011 by Endimion17] |
How can something that's free be expensive? And who needs about 7 kg of zinc? From where I stand waste anodes are a lot harder to get than spent
battery casings.
|
|
Arthur Dent
National Hazard
![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif) ![*](images/xpblue/star.gif)
Posts: 553
Registered: 22-10-2010
Member Is Offline
Mood: entropic
|
|
I understand the reflex of using the least expensive sources for chemicals, but depleted alkaline and C/Zn batteries is more wasteful of your time and
energy than anything. As the members above have posted, there are far better sources for these components.
1st thing is real carbon zinc batteries, I suggest that you go to a dollar store (do you have those in Italy?) and buy some fresh C/Zn D-cells, two
packs of two at a dollar a piece isn't bad. You'll get some Manganese dioxide that you can clean-up and purify (several threads here on that). The
casings are made of relatively pure zinc, and can be cleaned and cut in little bits. Finally, you have the rods that are made out of carbon and can be
used for electrolysis and stuff.
If you don't have such a store in your area, it's worth it to do a little trekking around town to find one. For example, just at my store near me, I
can get pure paraffin oil for lamps, pure sodium acetate in hand warmers, hydrogen peroxide, naphta, baking soda in bulk, ammonia, denatured alcohol,
zeolite, coffee filters, wire brushes, reagent jars and a ton of useful stuff... all for a dollar or two!
Robert
--- Art is making something out of nothing and selling it. - Frank Zappa ---
|
|
Demonblack
Harmless
Posts: 8
Registered: 23-11-2011
Location: Italy
Member Is Offline
Mood: No Mood
|
|
Quote: Originally posted by Arthur Dent ![](images/xpblue/lastpost.gif) |
1st thing is real carbon zinc batteries, I suggest that you go to a dollar store (do you have those in Italy?) and buy some fresh C/Zn D-cells, two
packs of two at a dollar a piece isn't bad. You'll get some Manganese dioxide that you can clean-up and purify (several threads here on that). The
casings are made of relatively pure zinc, and can be cleaned and cut in little bits. Finally, you have the rods that are made out of carbon and can be
used for electrolysis and stuff.
|
It's pointless and wasteful...
If i wanted to buy it, i'd go at the chemical shop (there's a relatively big one in Turin).
The thing about using depleted batteries is that they're not useful anymore, and their processing as special waste also costs money and energy.
Opening them with a pair of pliers doesn't ![;)](./images/smilies/wink.gif)
Oh, btw we do have the "1€" stores
Quote: |
If you don't have such a store in your area, it's worth it to do a little trekking around town to find one. For example, just at my store near me, I
can get pure paraffin oil for lamps
|
Also sold as baby oil (get the cheapest one so that it doesn't have any parfumes)
Quote: | pure sodium acetate in hand warmers
|
Never even heard of these, more info?
Quote: | , hydrogen peroxide,baking soda in bulk, ammonia, denatured alcohol
|
Pretty much everywhere lol
Lamp fuel, pretty hard to find these days
Quote: |
zeolite, coffee filters, wire brushes, reagent jars and a ton of useful stuff... all for a dollar or two!
|
I got some coffee filters for 0.7€, but they're crap. They tend to self-destruct much more easily than regular paper and also allow the finer
powders to pass trough. Avoid the "Aromata" brand...
Never saw zeolite around, but a lot of regular supermarkets sell sodium hydroxide in 500g packs for like 3€ or so. ![:P](./images/smilies/tongue.gif)
However i have trouble finding KCl, they sell it as salt subtitute but all the brands i saw are around the 7/3 KCl/NaCl ratio, no pure KCl...
|
|