Is this silicon ?


I heated a little bit of SiO2 sand with powdered charcoal in a stoiciometrcal 5:1 mass ratio (actually 6:1 to get a bit overdose of carbon) in an electric arc. The arc is made by a 80A welder with carbon rods and heats the stuff easily to over 2000oC. This results in:

SiO2 + C => Si (l) + CO2 (g)

In the picture (center where the arc occurred) very small globular particles can that be metallic Si ?
The SiO2 "melts" @ 1710oC but then it actually gets a sticky mass in which the Si droplets precipitate, but is this Si ??


View user's profile View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 19-11-2011 at 11:54


Could be: heavily contaminated with SiC of course...

Try and chisel one out of there: Si reacts well with strong alkali, giving hydrogen and silicate... It does look like it.

Oversized photo alert! Try cropping to the part that's most interesting: 75 % of this pic is junk.

[Edited on 19-11-2011 by blogfast25]




View user's profile View All Posts By User
metalresearcher
National Hazard
****




Posts: 737
Registered: 7-9-2010
Member Is Offline

Mood: Reactive

[*] posted on 19-11-2011 at 12:55


I put some particles into hot NaOH solution, but no gas escaped. So it is probably SiC. According to http://en.wikipedia.org/wiki/SiC this will form SiC and this substance is produced this way.
View user's profile View All Posts By User
Adas
National Hazard
****




Posts: 711
Registered: 21-9-2011
Location: Slovakia
Member Is Offline

Mood: Sensitive to shock and friction

[*] posted on 19-11-2011 at 14:48


So next time try to use less carbon.
View user's profile Visit user's homepage View All Posts By User
blogfast25
International Hazard
*****




Posts: 10562
Registered: 3-2-2008
Location: Neverland
Member Is Offline

Mood: No Mood

[*] posted on 20-11-2011 at 06:04


Quote: Originally posted by Adas  
So next time try to use less carbon.


Not really: the combination of silica and carbon at these temperatures tends to form SiC (which looks rather much like Si)